Abstract
Membranes are widely applied in water and wastewater treatment in the removal of a wide range of organic, inorganic, and biological pollutants. Despite their application, polyethersulfone (PES)‐based membranes are limited due to their hydrophobic nature; the inherent hydrophobicity restricts water transport, promotes membrane fouling, and reduces the effective removal of hydrophilic organic contaminants. This study systematically investigated the impact of hydrophilic additives (polyethylene glycol, glycerol and starch) on the structural properties, permeability, contaminant rejection, and antifouling and antimicrobial behavior of polyethersulfone (PES)‐based membranes. The additives produced distinct changes in membrane morphology, hydrophilicity, permeability, contaminant rejection, and fouling behaviour. Starch modification provided the highest rejection of ciprofloxacin (CIP), rhodamine B (RhB), and natural organic matter (NOM) (21.5%, 22.9%, and 67%, respectively), whereas glycerol provided the best antifouling performance (flux recovery ratio, FRR = 62.2%). PEG produced a highly porous membrane (94.95%) with a small estimated mean pore radius (2.2 nm), while the PEG/glycerol membrane exhibited the highest water permeability (1238 LMH). The ternary PEG/glycerol/starch formulation did not simultaneously improve membrane performance. Real water experiments further showed that NOM fouling affected contaminant rejection differently, with RhB rejection increasing whereas CIP rejection generally decreased after fouling. This study demonstrates that hydrophilic additive modification of PES membranes is an effective strategy for tuning membrane structure and performance, but the choice of additive and the decision to combine additives must be strategically aligned with the target application.
1 Introduction
Membranes are widely used in water treatment to remove organic, inorganic, and microbial contaminants. Their use has expanded globally, leading to improved performance and broader adoption in treating both drinking water and wastewater. However, the performance of polyethersulfone (PES)-based membranes is critically limited by their inherent hydrophobicity, resulting in low water permeability, rapid fouling, and poor rejection of hydrophilic organic contaminants. (Mahlangu et al., 2023). Hydrophilic additives including polyethylene glycol (PEG), glycerol, and starch are increasingly being incorporated into the PES matrix for improved membrane performance, largely by altering the membrane’s structure and morphology. PEG acts as a pore-forming agent that improves the membrane’s hydrophilicity, resulting in higher pure water flux and increased pollutant rejection. Studies have also reported improved water permeability and superior antifouling properties attributable to the integration of PEG (Ma et al., 2011; Alam et al., 2024). Glycerol, on the other hand, in addition to being a pore former, is also a plasticizer which offers membranes a more open and interconnected pore structure, thus improving overall water flux and hydrophilicity. Enhanced pollutant rejection, particularly the removal of proteins and other organic pollutants, has also been reported. Notably, glycerol-modified membranes exhibit reduced irreversible fouling due to the hydrophilic surface’s inability to restrain foulants (Su and Hiep, 2025; Paluch et al., 2022). The current study assesses the use of starch as an environmentally friendly membrane modifier. The hydrophilic surface of starch-modified membranes is anticipated to facilitate the formation of a hydration layer, which will subsequently act as a barrier against foulant deposition, thereby improving both flux recovery and membrane lifespan (Mudau et al., 2026; Saedi et al., 2013). PES-based membranes are also susceptible to biofouling. Hence, hydrophilic additives are expected to influence antibacterial activity through several mechanisms: (i) enhanced surface hydrophilicity which reduces bacterial adhesion; (ii) the introduction of functional groups (hydroxyl, amine, or ether) that can interact with cell membranes; (iii) formation of hydration layers that sterically hinder bacterial attachment (Phillip et al., 2026; Hassouna et al., 2025).
Research on combining different types of hydrophilic additives (PEG, starch, and glycerol) into the PES matrix to assess the effect of structure-performance remains limited. This work aims to improve understanding of how varying additives affect the membrane’s surface chemistry, pore size, and pore distribution, which are useful for predicting adhesion and contaminant rejection. Furthermore, fouling behavior and retention characteristics remain poorly characterized, which necessitates systematic studies to understand the role of hydrophilic additives in strategically modifying membranes for enhanced membrane performance (Adeniyi et al., 2023; Zhao et al., 2024). Alongside membrane advances, the water matrix plays a critical role, as most water sources are heavily contaminated with a diverse range of persistent organic contaminants, including pharmaceutical residues, synthetic dyes, and natural organic matter. Ciprofloxacin (CIP) is frequently detected in water and resists removal in conventional treatment processes because its zwitterionic nature limits electrostatic capture. Its fluorinated structure resists microbial degradation, and its solubility means CIP dissolves in water rather than partitioning into removable phases (Mabaso et al., 2026). Similarly, Rhodamine B (RhB) is highly soluble in water. Together with natural organic matter (NOM), these contaminants pose risks to human health and therefore require removal strategies in drinking water treatment.
Hydrophilic PES-ultrafiltration (UF) membranes are uniquely positioned to remove contaminants from water owing to the diversity of membranes’ contaminant removal mechanisms, including size exclusion, adsorption, cake layer formation, and electrostatic interactions. The rejection mechanisms are influenced by the physicochemical properties of the target contaminants and depend on the interplay of solute size, charge, and membrane surface chemistry (Foorginezhad et al., 2025). For CIP (331 g/mol, zwitterionic at pH 7.3), size exclusion is expected to be ineffective as its molecular dimensions (∼1.0–1.3 nm) are smaller than typical UF membrane pores (2–10 nm). Rejection is therefore expected to be governed by adsorption, primarily through hydrogen bonding between CIP’s functional groups and the membrane’s surface hydroxyl (O-H) groups, as well as hydrophobic interactions with the PES backbone (Enyoh and Wang, 2024). Incorporating hydrophilic additives is expected to enhance CIP rejection by increasing the density of hydrogen-bond donors on the membrane surface. For Rhodamine B (479 g/mol, cationic at pH 7.3), a combination of size exclusion and electrostatic attraction is expected. RhB’s larger size (∼1.5–1.8 nm) facilitates removal through size exclusion. Additionally, the positive charge facilitates electrostatic attraction to negatively charged membrane surfaces or anionic NOM fouling layers (Kuśmierek et al., 2023). For NOM fractions (500–2000 Da), a combination of size exclusion and adsorption will govern removal. Cake layer formation is also expected to play a significant role during prolonged filtration, wherein accumulated particles and macromolecules form a secondary porous layer that reduces effective pore size and enhances rejection of smaller contaminants. This dynamic layer is anticipated to be particularly influential in real water matrices, where accumulated NOM can enhance retention of cationic dyes like RhB while increasing hydraulic resistance. The presence of competing NOM may have dual effects; it can either compete with CIP for adsorption sites, reducing rejection, or enhance RhB rejection through electrostatic attraction and cake layer filtration (Peng et al., 2022; Liu et al., 2022).
In this study, PES membranes are modified using hydrophilic additives, and a systematic comparison of single, binary, and ternary combinations of PEG, glycerol, and starch is undertaken to understand their synergistic and antagonistic effects on membrane structure and performance. The study comprehensively investigates the impact of these additives on membrane morphology, structural properties, hydrophilicity, permeability, pollutant rejection, antimicrobial efficacy, and fouling behavior. This work emphasizes how additive interactions influence pore formation, surface chemistry, and membrane selectivity, and how real water NOM fouling affects the rejection of contaminants with different physicochemical characteristics, namely, cationic rhodamine B and zwitterionic ciprofloxacin. The anticipated rejection mechanisms are systematically evaluated through extensive membrane characterization and performance testing, with special attention given to the contribution of hydrogen bonding and surface chemistry as alternative pathways to conventional pore-size-controlled separation. By integrating experimental characterization with performance evaluation, this work aims to provide new insights into the rational design of next-generation PES ultrafiltration membranes with enhanced hydrophilicity, permeability, selectivity, and fouling resistance for water treatment applications.
2 Experimental methodology
2.1 Chemicals and materials
Polyethersulfone (PES, 58.000 g/mol) was obtained from Solvay Polymers. Polyethylene glycol (PEG-400), bovine serum albumin (BSA), ciprofloxacin (CIP), Rhodamine B, and N-Methyl-2-pyrrolidone (NMP), Mueller-Hinton (MH) agar and broth were obtained from Merck South Africa. Glycerol was obtained from RLS Chemicals South Africa, and starch (standard commercial variant) was acquired from Model Product Distributors. Deionized water was obtained from the Elix integral-10 water purification system (Merck Millipore). We purchased Staphylococcus aureus ATCC 25923 from KWIK-STIK™, a product line of Microbiologics®, South Africa. The real water samples were collected from a lake in South Africa from three sampling sites (inlet, middle, and the outlet), using the grab sampling method as per Mabaso et al. (2026), wherein 1 L Schott glass bottles were used and immediately placed in an ice-filled chiller for preservation during transportation. The samples were then stored in a chiller at 4 °C, and the water was used without pretreatment (Mabaso et al., 2026).
2.2 Fabrication of membranes with hydrophilic additives
Six PES flat-sheet membranes were fabricated using the phase inversion method described in a previous study by Tshangana et al., with minor changes (Table 1) (Tshangana and Muleja, 2024). PES was dissolved in NMP at room temperature while stirring at a constant speed of 300 rpm for 12 h until a homogeneous solution was obtained. The additives (PEG and glycerol) were then added individually. Starch, on the other hand, was first mixed with water to improve its dispersion in the casting solution and subsequently added to the casting solution. All casting solutions containing different additives were stirred at a constant speed of 300 rpm at 40 °C for 6 h until homogeneous solutions were formed. The homogeneous casting solutions were kept in a dark cabinet overnight for degassing. The resultant homogeneous casting solutions were spread evenly on a glass plate at 28 °C using a casting knife to achieve a uniform film thickness (200 µm). The cast films were immediately immersed in a water bath to initiate phase separation. The resultant membranes were thoroughly washed to remove residual solvent and additives, and were then stored in water until preserved for characterization and application. The washing step was intended to remove loosely bound and unincorporated additives from the membrane matrix. However, this study did not quantitatively evaluate additive release during prolonged aqueous exposure.
TABLE 1
| Membrane ID | PES (w%) | NMP (w%) | PEG (w%) | Glycerol (w%) | Starch (w%) | Deionized water (w%) |
|---|---|---|---|---|---|---|
| PES | 18 | 82 | 0 | 0 | 0 | 0 |
| PES/Gly | 18 | 80 | 0 | 2 | 0 | 0 |
| PES/PEG | 18 | 62 | 20 | 0 | 0 | 0 |
| PES/Starch | 18 | 80 | 0 | 0 | 1 | 1 |
| PES/Gly/PEG | 18 | 60 | 20 | 2 | 0 | 0 |
| PES/Gly/PEG/Starch | 18 | 58 | 20 | 2 | 1 | 1 |
Composition (wt%) of fabricated membranes used in the study.
2.3 Characterization of the fabricated membranes
The functional groups of the resultant membranes were characterized with a Fourier-transform infrared (FTIR) spectrometer (Frontier PerkinElmer, Spectrum 100 spectrometer, Waltham, MA, USA). A scanning electron microscope equipped with energy-dispersive X-ray spectroscopy (SEM/EDS) (JSM-7800 F JEOL JEM-2100, Tokyo, Japan) was used to assess the morphological characteristics and elemental composition of the fabricated membranes. Atomic force microscopy (AFM) (Alpha300A, WITec, GmbH, Ulm, Germany) in non-contact mode was used to assess the membranes’ surface morphology and roughness (Sa). The hydrophilicity of the fabricated membranes was analyzed by measuring the water contact angle (WCA) using a goniometer (DSA30, Krüss GmbH, Hamburg, Germany). We measured the average WCA using the static sessile drop method with a 2 µL volume. For bulk porosity and pore size measurements, the gravimetric method was used. The membranes were cut into 2 cm × 2 cm specimens and soaked in water for at least 24 h to ensure that the membrane pores were filled with water. The membrane surface was gently wiped to remove excess surface water and weighed. The membranes were then dried in an oven at 60 °C for 2 h and weighed again. The bulk porosity (ε) was then calculated using Equation 1 (Nhlengethwa et al., 2024).where and are the weights of the wet and dry membranes (g), respectively. is the area of the membranes (4 cm2), is the thickness of the membranes (cm), and is the density of water (0.998 g/cm3).
The average pore size of the membranes ( was determined using the Guerout–Elford–Ferry Eq (Equation 2). using the filtration method (Nhlengethwa et al., 2024).where is pure water flux (m/s), is the water viscosity (8.9 × 10−4 Pa·s) and is the operating pressure (3 bar = 300,000 Pa).
The mechanical properties of the membranes were examined using Small-Angle X-ray Scattering (SAX Space) equipment (Anton Paar, Graz, Austria) with a tensile stage to measure strain and elongation.
The surface charge of the membranes was estimated using the pH point of zero charge (pHPZC). The pH drift method was used to measure the pHPZC of the pristine and modified membranes. Membrane pieces, measuring 1 cm by 1 cm, were immersed in 12 mL of 0.01 M KCl, and the initial pH was adjusted to the desired pH range (2–12) using either 0.1 M NaOH or 0.1 M HCl. After pH adjustment, the solutions were shaken at 150 rpm (Labcon CPB450, Johannesburg, South Africa) at room temperature for 24 h, after which the final pH (measured using a pH meter, Seven Direct SD20, Mettler Toledo, Malaysia) was recorded. To obtain the membrane pHPZC values, the final pH values were plotted against the initial pH values.
2.4 Performance of membranes
2.4.1 Membrane permeability
The pure water flux (PWF) of the membranes was evaluated by permeating pure water using a dead-end system with an active membrane area of 0.00126 m2. Water permeation was determined by measuring the volume of water permeated by the membranes in 10 min at different pressures (1–5 bar). The membranes were first compacted at 6 bar until a steady flux was achieved. Equation 3 was applied to calculate the water flux (Chakachaka et al., 2023).where = Flux (L·m-2·h-1), = permeate volume (L), = active membrane area (m2), = time(h).
2.4.2 Removal of organic contaminants in lake water using the fabricated membranes
The rejection of NOM from the Florida water sample was determined using the Aqualog-UV-800 (Aqualog, HORIBA, Jobin Yvon, USA) instrument. The UV254 absorbance and fluorescence excitation-emission matrix (FEEM) of real water were measured between 200 nm and 800 nm at 2 nm excitation intervals and emission wavelengths between 248.58 nm and 830.59 nm at 3.28 nm emission intervals. The rejection was then calculated using Equation 4 (Nhlengethwa et al., 2025).where = Rejection of organics (%), = Fluorescence intensity in the permeate = Fluorescence intensity (or integrated fluorescence) in the feed.
2.4.3 Removal of ciprofloxacin using the fabricated membranes
A stock solution was prepared by dissolving 5 mg of CIP in 10 mL of 0.1 M HCl. The solution was then transferred to a 1 L flat-bottom flask. Deionized water was added to the mark, and NaOH was used to adjust the pH to 7.3, which is the isoelectric pH of CIP (Horká et al., 2014). The 5 mg/L CIP concentration was selected as a model concentration consistent with several laboratory-scale studies investigating membrane-based CIP removal. Such concentrations facilitate reliable analytical quantification and enable comparison of membrane–solute interactions and separation mechanisms (Hawa et al., 2013; Al-Shaeli et al., 2026; Zazouli et al., 2008). CIP rejection was determined from the concentrations measured in the feed and permeate solutions after filtration at an operating pressure of 3 bar using the dead-end filtration cells. The concentration of CIP in the feed and permeate was determined by measuring the absorbance of filtrate at the wavelength of maximum absorption (λ = 277 nm) using a UV–Vis Spectrophotometer (Perkin Elmer UV–Vis spectrometer Lambda 6,505). The CIP removal was determined using Equation 5 (Tshangana, 2022).where Cf and Cp represent the concentrations of the feed and the permeate, respectively.
The experiment was repeated using real water samples collected from the lake and spiked with CIP (5 mg/L) to determine the effect of competing species on rejection. To determine the effect of fouling on rejection, real water samples were filtered for 60 min until a cake layer was visible on the membrane surface. Subsequently, the prepared CIP solution was filtered and analyzed, and Equation 5 was used to calculate rejection.
2.4.4 Removal of rhodamine B using the fabricated membranes
The feed solution was prepared by dissolving 10 mg of RhB in 1 L of deionized water. This RhB concentration was selected as a model concentration commonly used in laboratory-scale treatment studies, not because 10 mg/L RhB has been established as a typical measured concentration in environmental wastewater (Matebese et al., 2025; Tripathi et al., 2014; Yildiz and Manzak, 2024). The solution was filtered using the dead-end filtration cells at 3 bar, and the permeate was collected. The rejection efficiency of the membranes was determined by analyzing the permeate using UV–Vis Spectroscopy (PerkinElmer UV–Vis spectrometer Lambda 6,505) to measure absorbance at 554 nm. The procedure was repeated using RhB dissolved in real lake water to determine the effect of competing species. Fouled membranes were also used in filtration to determine the effect of fouling on rejection. In these experiments, Equation 5 was also used to determine rejection.
2.4.5 Antifouling behavior of the modified membranes
A BSA solution (500 ppm; pH∼7) was used as a model fouling agent, and the antifouling performance of the membranes was evaluated by first conducting the pure water flux () for 30 min at 3 bar, followed by the flux of BSA () solution, which was measured for 30 min. Thereafter, the membrane was backwashed with deionized water for 30 min at 4 bar. After backwashing, the pure water flux () was measured again for 30 min. To evaluate fouling resistance, the flux recovery ratio () was calculated by applying Equation 6.
To analyze the fouling in detail, the total fouling (), reversible fouling (), and irreversible fouling () were evaluated by employing the following Equations 7–9, respectively (Hainiza Abd-Razak et al., 2020).
The flux reduction was also determined by filtering real water samples at 3 bar and collecting permeate for 1 min at 30-min intervals over 3 h. Flux was determined using Equation 3, and the percentage flux drop was determined using Equation 10 (Kouhestani et al., 2019):
2.4.6 Antimicrobial experiments
A single colony of Staphylococcus Aureus, a bacterial strain, was inoculated into Mueller-Hinton broth. The culture was incubated for 24 h at 37 °C with gentle shaking until mid-log phase (OD600 = 0.6). The antibacterial efficacy of the membranes was evaluated on Mueller-Hinton agar plates using bacterial suspensions (grown in a bacterial lawn) with turbidity corresponding to the 0.5 McFarland standard. 20 μL of the bacterial suspension was evenly spread over the Mueller-Hinton agar, and sterile membrane blank discs were placed on the surface of the inoculated plate, and the plates were incubated for 24 h at 37 °C. Zones of inhibition (distance from the disc circumference in mm) were measured for each disc in areas where no bacterial growth was observed (Kedang et al., 2022).
The anti-adhesion properties of the membranes against S. aureus were evaluated using a viable-cell enumeration method. The bacterial suspension was standardized to 5 × 105 CFU/mL, and membrane samples (1 × 1 cm) were immersed in it. After 1, 6, and 24 h of incubation at 37 °C, membrane samples were aseptically removed and gently rinsed to remove loosely attached bacteria. Each membrane was then transferred into 1 mL of sterile PBS and vortexed to detach viable bacteria from membrane surfaces. The recovered bacterial suspensions were serially diluted, and 20 µL aliquots were plated onto Mueller–Hinton agar. Following incubation at 37 °C for 24 h, colonies were counted and bacterial adhesion was expressed as CFU/cm2 using Equation 11. The anti-adhesion performance of the modified membranes was evaluated relative to the unmodified PES membrane.
2.5 Quality control and statistical analysis
All experiments were conducted in triplicate to ensure reproducible, accurate results. The results are reported as mean values with corresponding standard deviations. To evaluate the statistical significance of differences between treatment groups, a one-way analysis of variance (ANOVA) was performed. A p-value of less than 0.05 was considered indicative of a statistically significant difference. Where applicable, error bars in the figures represent standard deviations from the three independent experimental replicates. The triplicate measurements represent technical replicates from the prepared membrane samples and do not constitute independent fabrication batches; therefore, this study could not quantitatively assess batch-to-batch fabrication reproducibility.
3 Results and discussion
3.1 Characterization of membranes
3.1.1 Functional groups and elemental composition of membranes
The membranes were washed before characterization and application, although we did not quantitatively measure PEG, glycerol, or starch release into the wash water or permeate. The complete retention of the additives cannot be experimentally confirmed, and the observed differences in membrane performance are interpreted as the combined effect of additive incorporation, phase-inversion-induced morphological changes, and the possible redistribution or partial loss of the additives during membrane preparation and filtration. The surface characterization results provide evidence of the intended functional groups in the prepared membranes that were not leached completely during phase inversion and washing. The membranes were characterized for different physicochemical properties. Figure 1a shows the EDS graphs for the elemental composition of the membranes. All fabricated membranes contain S, C, and O, which are characteristic of the elemental PES membrane (Zhang et al., 2024). PES is generally expected to have the lowest surface carbon (C) and oxygen (O) contents, while the sulfur (S) content decreases significantly compared with membranes with additives. This can be attributed to the chemical structures of the additives (glycerol, PEG, and starch), which are rich in C and O. When these additives are blended into the casting solution. The membrane is formed, they are expected to migrate toward the membrane surface due to their hydrophilicity and lower molecular weight compared to PES (Gumbi, 2019; Shirzadeh-Gharacheh and Rahbari-Sisakht, 2016). The pristine PES membrane (PES) showed high carbon (83.95 wt%) and sulfur (11.66 wt%) content, consistent with the PES backbone. The modified membranes GLY–PEG/Gly/Starch exhibited dramatically lower carbon (39.75–44.36 wt%) and sulfur (7.98–9.21 wt%) content, confirming successful surface enrichment of the hydrophilic additives (glycerol, PEG, and starch) during phase inversion. The GLY, PEG, and PEG/Gly modified membranes showed nearly identical compositions (C: 43.5 wt%, O: 15.9 wt%, S: 8.7 wt%, O/C: 0.37), indicating comparable levels of surface enrichment despite their different performance characteristics. Starch-modified membranes, by contrast, showed slightly higher sulfur content (9.21 wt%) and a lower O/C ratio (0.34), suggesting that starch’s larger molecular size may limit its surface migration compared with glycerol and PEG. The PEG/Gly/Starch-modified membranes showed the lowest carbon (39.75 wt%) and sulfur (7.98 wt%) content, indicating the greatest dilution of the PES surface by additives (Gumbi, 2019). The FTIR spectra in Figure 1b show broad bands between 3,200 and 3,600 cm-1, ascribed to O-H functional groups in all membranes and indicative of surface hydrophilicity. The observed peaks in the range 1147-1151cm-1 and 1,104–1,105 cm-1 are attributed to the C-O and C-O-C stretching, respectively, which improves the surface water affinity of the membranes (Sałacińska et al., 2024). Another significant band affecting membrane surface properties, as observed, is the O=S=O broad band between 1,333 and 1,277 cm−1, which influences membrane polarity (Manawi et al., 2017). In these graphs, peak intensities decrease relative to PES, suggesting changes in functional group content in the membranes. The changes in FTIR peaks align with changes in surface morphology, indicating that chemical modifications are directly impacting the physical structure of the membrane (Lalia et al., 2013).
FIGURE 1
3.1.2 Morphology evaluation of the fabricated membranes
The SEM cross-sectional images (Figure 1d and inserts) of all the membranes reveal the typical asymmetric structure characteristic of phase-inverted PES membranes, while the AFM (Figure 1d) shows the surface roughness of the membranes. The SEM micrographs display a dense, thin top layer (skin) supported by a thicker, porous sub-layer with a finger-like morphology. This structure is consistent with the literature and is essential for achieving both selectivity and high permeability in ultrafiltration and microfiltration membrane applications (Gayatri et al., 2023). The top layer of the pristine PES membrane is relatively dense and thicker than that of the modified membranes, and exhibits moderate surface roughness (sa = 63.1 nm) attributable to the slower solvent–non-solvent exchange during immersion precipitation because the absence of hydrophilic additives delays water influx (Wen et al., 2022). The PES membrane also has visible, moderately developed finger-like macrovoids that are irregular in length and width. The macrovoids originate from the instantaneous demixing at the top surface. The growth is not as extensive as in additive-containing membranes because the casting solution lacks hydrophilicity-enhancing agents that promote rapid solvent outflow and water inflow (Ma et al., 2011; Koo et al., 2025). Glycerol-modified membranes were significantly thinner and exhibited more elongated and relatively uniform finger-like macrovoids than the pristine PES membrane. The incorporation of glycerol alters the thermodynamic and kinetic characteristics of the casting solution during nonsolvent-induced phase separation, promoting more rapid demixing and precipitation. Glycerol can also modify the interfacial interactions between the polymer solution and the coagulation bath, facilitating water penetration into the polymer-rich phase. Since finger-like macrovoids are associated with rapid nonsolvent transport into the casting solution, enhanced nonsolvent influx can promote their development and propagation through the membrane sub-layer (Mamba et al., 2024). This accelerates demixing at the top surface, resulting in a thinner skin with increased roughness (sa = 84.4 nm). The top layer of PEG-modified membranes is extremely thin and visibly discontinuous in some regions and is also the most porous amongst the fabricated membranes. The PEG-modified membranes have highly developed finger-like macrovoids among all membranes because PEG-400 is a low-molecular-weight, highly water-soluble pore former that rapidly leaches out into the coagulation bath during phase inversion, leaving behind a highly porous structure with the greatest surface roughness (sa = 209.6 nm) and a very thin skin layer. The top layer of starch-modified membranes is noticeably thinner than the PES-modified membranes but denser and more uniform than Gly and PEG membranes. The shorter, more uniform, and less elongated finger-like macrovoids compared to Gly and PEG are a result of starch enhancing the viscosity of the casting solution significantly, slowing down the diffusion of solvent out of the film and non-solvent into the film. This leads to a more controlled, delayed demixing at the top surface, producing a tighter skin layer and hindering the rapid growth of large macrovoids, resulting in smaller, more sponge-like pores. This induced viscosity, which promotes uniform skin formation, also caused starch to have the smoothest surface with an SAof 29.9 nm (Mamtora and Kurada, 2025). The combination of PEG (leachable pore former) and glycerol (plasticizer/hydrophilicity enhancer) synergistically promotes rapid water influx and additive leaching, resulting in a highly porous and minimal skin layer. This leads to PEG/Gly membranes having an extremely thin, smooth skin (sa = 88 nm) comparable to PEG membranes, and the most pronounced and longest finger-like macrovoids of any membrane. Starch may increase the resistance to mass transport within the casting solution, potentially slowing solvent–nonsolvent exchange and delaying phase separation, whereas glycerol may promote more rapid solvent–nonsolvent exchange and earlier demixing. This creates a competing effect, where PEG and glycerol accelerate demixing, and starch delays it. The net result is a skin layer of intermediate thickness in PEG/Gly/Starch, thicker than PEG/Gly but thinner than PES. Some irregularities and partial collapse of macrovoids in PEG/Gly/Starch are visible, likely due to the incompatible effects of starch (viscosity increase, delayed demixing) with PEG and glycerol. The membrane also showed a smooth surface (41.2 nm) due to the smoothing effect of starch, although the presence of starch appears to counteract the rapid demixing effects of PEG and glycerol, preventing it from achieving the smoothness observed for the starch-only membrane.
3.1.3 Contact angle, bulk porosity, and mean pore size determination of the fabricated membranes
Contact angle measurements were performed to assess the hydrophilicity or hydrophobicity of the membranes, with a lower contact angle indicating greater hydrophilicity. Generally, membranes with higher surface hydrophilicity are better at attracting water molecules and preventing the adsorption of contaminants. This is beneficial for enhancing water flux and preventing fouling, and the rejection of hydrophobic contaminants (Nhlengethwa et al., 2024). Water contact angle measurements revealed significant differences in surface hydrophilicity across the membranes (Figure 2a). Pristine PES membranes exhibited the highest contact angle (68.68°), consistent with its FTIR spectrum showing the lowest O-H band intensity (highest transmittance of 70%) and EDS confirming the absence of oxygen-rich additives, while SEM revealed a relatively dense skin layer without surface-enriched hydrophilic domains. The incorporation of glycerol (60.31°) and PEG (56%) progressively reduced the contact angle, correlating with increased O-H and C-O FTIR band intensities, higher surface oxygen content by EDS (O/C ratio 0.37), and SEM-observed thinner skin layers from accelerated demixing. Starch achieved the lowest contact angle (43.65°), which is attributed to starch’s abundant hydroxyl groups as confirmed by FTIR (lowest O-H transmittance of 67%), the highest surface enrichment of oxygen-rich polysaccharide, and AFM revealing the smoothest surface topography (29.9 nm), a result of starch-induced viscosity increase promoting controlled, delayed demixing. PEG/Gly (PEG + glycerol, 50.31°) showed a contact angle intermediate between PEG and Starch membranes, reflecting synergistic surface enrichment of both additives (O/C ratio 0.37) despite SEM observations showing near-instantaneous demixing and the longest macrovoids. PEG/Gly/Starch exhibited a contact angle of 52.90°, higher than both STARCH and PEG/Gly despite containing all three additives. This provides quantitative evidence that the combined additives did not yield the expected improvement in hydrophilicity, suggesting that the additives may compete for surface sites rather than cooperatively enriching the membrane interface. FTIR showed less O-H reduction than Starch membrane, EDS revealed the highest additive dilution (lowest C and S) but not the highest O/C ratio, and SEM confirmed irregular macrovoids with partial collapse, indicating that starch, PEG, and glycerol compete for surface sites rather than cooperatively enriching the interface (Matebese et al., 2025). The contact angle trend (Starch < PEG/Gly < PEG/Gly/Starch < PEG < Gly < PES) demonstrates that surface hydrophilicity is governed by the chemical nature, molecular mobility, and combined interactions of additives during phase inversion, not merely by their presence or total concentration, with starch producing the most hydrophilic surface through its multivalent hydroxyl structure and controlled demixing kinetics (Jason Kwong, 2017; Qalyoubi et al., 2022).
FIGURE 2
The gravimetric method was used to determine the bulk porosity, while the mean pore radius was calculated using water permeation data. The porosity and pore radius data in Figure 2b correlate directly with the SEM-observed morphologies. PEG achieved the highest porosity (94.95%) due to the leaching of PEG-400, but the smallest mean pore radius (2.2 nm) because skin pores are templated by individual PEG molecules. This high porosity mainly reflects the highly porous sub-layer formed during phase inversion, while the calculated pore radius represents the average pore size in the selective skin layer. Thus, a membrane can simultaneously exhibit high bulk porosity (due to macrovoids) and small skin layer pores. PEG/Gly exhibited the largest mean pore radius (7.5 nm) despite only moderate porosity (67.14%), consistent with its SEM showing the longest macrovoids and a highly open skin from synergistic PEG + glycerol effects. Starch and Gly membranes both showed moderate porosity (70.64% and 69.22%) but achieved this through different mechanisms, glycerol via accelerated demixing (Gly), and starch via viscosity-controlled, delayed demixing. The ternary membrane PEG/Gly/Starch displayed intermediate properties (74.12% porosity, 6.4 nm radius) with irregular SEM morphology, confirming combined interactions between starch and the smaller additives. These results demonstrate that bulk porosity and mean pore radius are independently tunable through strategic additive selection, but combining multiple additives does not guarantee superior structural properties.
3.1.4 Mechanical strength of the fabricated membranes
The mechanical performance of the membranes is illustrated in Figure 2c, specifically their tensile strength and elongation at break. Tensile strength is the maximum stress that a membrane can withstand while being stretched/elongated. Upon the incorporation of PEG, glycerol, and starch, a general trend of reduced tensile strength compared to PES is observed, which is typical when hydrophilic or pore-forming additives are introduced, as they tend to disrupt the dense polymer matrix and increase porosity (Afzal et al., 2024; Tsolele et al., 2025). The mechanical properties of the fabricated membranes are directly governed by their cross-sectional morphology, as observed by SEM. PES, with a relatively dense selective layer and moderately porous meso-layer, exhibited the highest tensile strength (0.71 MPa) but only moderate elongation (8.6%). The introduction of glycerol (Gly) and PEG produced thinner skin layers and elongated finger-like macrovoids, which reduced tensile strength to 0.61 MPa and decreased elongation to 5.8%, indicating brittle failure due to stress concentration at macrovoid tips. In contrast, Starch-modified membranes (starch only) displayed a sponge-like meso-layer with shorter macrovoids, resulting in the highest elongation (20.1%) while tensile strength was 0.65 MPa, demonstrating that a compact, uniform structure enhances ductility despite presenting greater resistance to water flow. The PEG/Gly membranes, on the other hand, had the most open channel structure and the highest flux but suffered the lowest tensile strength (0.59 MPa), confirming the inverse relationship between permeability and mechanical robustness. Whereas the PEG/Gly/Starch membranes exhibited intermediate properties (0.67 MPa, 10.3% elongation), reflecting the combined effects of combining rapid-demixing agents with viscosity-modifying starch. These results confirm that the selective layer and meso-layer architecture, whether they consist of open macrovoids or compact sponge-like structures, dictate both the hydraulic resistance and the mechanical resilience of the membrane (Ilomäki, 2023).
3.1.5 Membrane surface charge
The surface charge behaviour of the prepared membranes was evaluated using the pH-drift method, and the corresponding results are presented in Figure 3. The estimated points of zero charge (pHPZC) of the membranes ranged from approximately 6.59–6.94, indicating that the surface charge transition for all membranes occurred close to neutral pH. Pristine PES exhibited a pHPZC of approximately 6.67, while incorporation of glycerol and PEG shifted the estimated pHPZC to 6.84 and 6.94, respectively. The PEG/Gly membrane similarly exhibited a relatively higher pHPZC of approximately 6.91. In contrast, the starch-containing membranes exhibited slightly lower values of approximately 6.62, while the fouled membrane showed the lowest estimated pHPZC of approximately 6.59. These variations indicate modest changes in the interfacial acid–base and charge characteristics of the membrane surfaces following additive incorporation and exposure to real water. Since all estimated pHPZC values were below neutral pH, the membrane surfaces are expected to exhibit predominantly negative character at pH 7.
FIGURE 3
3.2 Membrane performance
3.2.1 Pure water flux of the fabricated membranes
The pure water flux results in Figure 2d correlate strongly with the structural characteristics of the membranes, which govern the rate at which water passes through the membrane. The pure water permeability of all tested membranes increased with an increase in pressure, attributable to the enhanced driving force associated with higher pressure conditions (Saravia and Frimmel, 2008). The addition of hydrophilic additives improved the permeability of the membranes relative to PES as expected. The improved porosity and hydrophilicity of the membranes enabled them to absorb and allow water penetration more easily (Alam et al., 2024; Su and Hiep, 2025). Between 1 and 2 bar, PES and Gly, PEG and Starch, and PEG/Gly and PEG/Gly/Starch had almost similar flux, a clear distinction was first observed at 3 bar in PES, Gly, PEG and Starch, and at 4 bar in PEG/Gly and PEG/Gly/Starch. PES membranes had the lowest flux (323.8 L/m2h at 5 bar) due to its thick, hydrophobic skin (68.68°) and lowest porosity (63.36%). The Gly-modified membranes (600 L/m2h) illustrated that open macrovoids improve flux over compact structures, but their moderate pore size (4.8 nm) and brittleness (6% elongation) limited performance. PEG/Gly membranes, on the other hand, achieved the highest flux (1238 L/m2h) at 5 bar due to the largest mean pore radius (7.6 nm) and the most open macrovoid structure from synergistic PEG + glycerol effects, though this came at the cost of the lowest tensile strength (0.59 MPa). The larger effective pore radius provides less hydraulic resistance to water transport. PEG, despite having the highest porosity (95%), exhibited only moderate flux (838.1 L/m2h at 5 bar) because its mean pore radius was the smallest (2.2 nm), demonstrating that skin layer pore size, not bulk porosity, is the rate-determining factor for flux. Thus, high bulk porosity does not necessarily result in high water permeability. The higher flux of PEG/Gly compared to PEG, despite PEG having higher bulk porosity (94.95% vs. 67.14%), is explained by the rate-determining role of skin layer pores. According to the Hagen-Poiseuille Eq., flux through pores scales with the fourth power of pore radius (). The 3.5-fold larger skin pores of PEG/Gly (7.6 nm vs. 2.2 nm) result in approximately 150-fold higher flow per pore, more than compensating for its lower bulk porosity. Additionally, the extremely thin skin layer of PEG/Gly membranes (observed in SEM, Figure 1D) minimizes resistance by reducing the flow path length. PEG/Gly/Starch (1133 L/m2h) achieves the second-highest flux through a combination of high porosity (74%) and large pores (6.4 nm), with balanced mechanical properties (0.67 MPa, 10% elongation), though antagonistic interactions with starch reduce its surface hydrophilicity. These results confirm that flux is governed by a combination of skin layer thickness, skin pore size, surface hydrophilicity, and sub-layer morphology, with the smallest constriction in the flow path typically the skin layer controlling the overall hydraulic resistance (Kaszás et al., 2013). Changes in additive retention during prolonged filtration could also influence membrane hydrophilicity and consequently affect long-term permeability. Therefore, additive stability may also influence the consistency of solute rejection during extended operation.
3.2.2 Ciprofloxacin rejection using the fabricated membranes
The rejection and removal mechanism of the fabricated PES membranes are depicted in Figures 4a‐d, the membranes exhibited low CIP rejection, ranging from 9.5% to 21.5% (Figure 4a) in deionized water. The highest rejection was obtained with the starch‐modified membrane (21.5%), whereas the pristine PES membrane showed the lowest rejection (9.5%). CIP is a zwitterionic antibiotic (MW 331 g/mol, pKa1 ∼6.2, pKa2 ∼7.9) with molecular dimensions between 1‐1.3 nm, which are smaller than the pore radii of all membranes investigated in this study. CIP molecules can easily pass through the membranes’ pores, ruling out size exclusion as a possible dominant rejection mechanism in the removal of CIP (Ignaciode Leon and Zharov, 2011). This shows that bulk porosity does not explain the observed rejection, with retention likely influenced by the selective skin‐layer characteristics and membrane surface chemistry (Lagiewka et al., 2024). At the experimental pH, CIP predominantly exists in its zwitterionic form, containing both positively and negatively charged functional groups. Although electrostatic interactions may contribute to CIP retention due to the membrane surface charge, the zwitterionic nature of CIP reduces the likelihood of a single dominant electrostatic repulsion mechanism. Consequently, non-electrostatic interactions, particularly hydrogen bonding between the polar functional groups of CIP and oxygen‐containing groups on the modified PES membrane surface, contribute substantially to its retention (Figure 4c). The incorporation of PEG, glycerol and starch introduces additional oxygen-containing functionalities onto the PES membrane surface, as indicated by the FTIR and EDS results in Figure 1. These functionalities provide hydrogen-bonding sites for CIP through interactions involving its carboxyl and piperazine-containing groups, leading to CIP retention. Similar interactions between CIP and oxygen-/nitrogen-containing functional groups on modified membrane surfaces have been reported, with hydrogen bonding identified as an important contributor to CIP removal (He et al., 2023). The increased hydrophilicity of the modified membranes may also alter the hydration layer and the balance between CIP–water and CIP–membrane interactions; however, enhanced hydrophilicity does not necessarily imply stronger CIP adsorption because CIP remains highly water-soluble. Adsorption may therefore contribute to CIP retention through interactions between CIP functional groups and polar membrane sites, although the relatively low rejection values indicate that these interactions were insufficient to provide strong overall retention under the conditions investigated. The highest CIP rejection (21.5%) was observed for the starch-modified membranes, this was attributed to high density of O-H groups (lowest transmittance) corroborated by FTIR in Figure 1d. The multivalent hydroxyl structure of starch-modified membranes provides multiple potential hydrogen-bonding sites for interaction with CIP, which may enhance solute–membrane affinity and contribute to the higher observed retention (Mantel et al., 2021). The literature reports significantly higher CIP rejections (77%–99.7%) with functional additives such as biochar, ZrP nanoparticles, and enzymes. Those studies use adsorption and photocatalysis in addition to filtration, whereas PEG, glycerol and starch are simple hydrophilicity modifiers and pore-formers without specific CIP-affinity groups (Pan et al., 2025; Yu et al., 2026).
FIGURE 4
3.2.2.1 The effects of competing NOM on CIP rejection
NOM in real water altered CIP removal, but removal remained dependent on membrane structure and rejection mechanisms. In contrast to the relatively low and consistent CIP rejection observed in deionized water (9.5%–21.5%), exposure to real water produced membrane-dependent changes in rejection. These changes indicate that NOM can modify the effective membrane pore structure and surface chemistry, thereby either enhancing physical retention or competing with CIP for surface interaction sites. PEG-modified membranes uniquely exhibited improved CIP rejection in real water, increasing from 13.5% to 24.5%. This increase was attributed to NOM components constricting the already small pores (2.2 nm) and creating a dynamic filtration layer that enhances size exclusion, a phenomenon not observed in any other membrane. However, after the membrane was subjected to the fouling condition, CIP rejection decreased to 11.5%, only slightly below the initial value of 13.5%. This indicates that the temporary enhancement observed during real-water filtration did not translate into a permanent improvement in selective rejection. The persistent NOM layer may have altered the membrane surface and transport pathways in ways that reduced of the interactions responsible for CIP retention. The relatively small change compared with the starch membrane suggests that the PEG membrane relies less on specific surface interactions and more on its relatively small pore size for the limited CIP retention observed. The starch-based membranes exhibited the largest declines, with rejection decreasing from 21.5% to 5.5% due to competition for hydrogen-bonding sites by NOM, and an 18.5% loss after real water fouling (21.5%–3.0%) as accumulated NOM blocked the hydroxyl groups responsible for CIP binding (Gong et al., 2023; Arahman et al., 2026). This reveals the fundamental vulnerability of adsorption-based rejection mechanisms: although they can achieve high clean-water rejection, they are unsustainable in complex real-water matrices where competing NOM largely occupies active sites. The Gly-based membranes showed large losses (15% in real water, 10.5% after real-water fouling) despite good hydrophilicity, indicating that glycerol’s hydration layer does not prevent competitive binding of soluble NOM to CIP interaction sites.
3.2.3 Rejection of rhodamine B using the fabricated membranes
Rhodamine B (RhB) (MW 479 g/mol) is a model contaminant found in various industrial wastewaters, such as that from the textile, leather, and paper industries. The rejection of RhB was also low, ranging from 9% to 22.9% (Figure 4b), following the trend Starch (22.9%) > PEG (21.2%) > Gly (18.8%) > PEG/Gly (14.6%) > PEG/Gly/Starch (10.9%) > PES (9.0%). Comparison with CIP rejection indicates that the relative contribution of the rejection mechanisms is influenced by the molecular characteristics of the solute and the structural and surface properties of the membrane (Figures 3c,d). RhB has larger molecular dimensions (approximately 1.5–1.8 nm) than CIP (approximately 1.0–1.3 nm), and therefore its transport through the membrane can be more strongly influenced by steric effects. This is evident from the higher RhB rejection (21.2%) than CIP rejection (13.5%) obtained with the PEG membrane, suggesting that the relatively smaller estimated pore size of the PEG membrane may provide greater steric resistance to the larger RhB molecule (Wang et al., 2026; Ang et al., 2020). The Starch membrane exhibited the highest rejection for both RhB (22.9%) and CIP (21.5%), despite its relatively larger estimated pore size (4.8 nm), indicating that surface-mediated interactions may contribute to solute retention in addition to steric effects. The incorporation of starch introduces abundant hydroxyl-containing functionalities, as indicated by the FTIR results (Figure 1b), which provide potential sites for hydrogen bonding with the polar functional groups of RhB and may increase solute–membrane affinity (Nilssen et al., 1996). At the experimental pH of 7, RhB is predominantly present in its cationic form, while the estimated pHPZC values of the membranes are below pH 7, indicating that the membrane surfaces are expected to possess a net negative charge under the experimental conditions. Electrostatic attraction between positively charged RhB and the negatively charged membrane surface may therefore contribute to RhB retention. The PEG/Gly membrane exhibited moderate RhB rejection (14.6%), which may be associated with its relatively large estimated pore size (7.6 nm), providing limited steric resistance to the larger RhB molecules, together with changes in surface chemistry and hydrophilicity caused by the combined additives. The PEG/Gly/Starch membrane exhibited lower RhB rejection (10.9%) than CIP rejection (15.5%), which may reflect the larger molecular size of RhB and differences in the accessibility and distribution of surface functional groups, as well as the heterogeneous membrane morphology produced by combining PEG, glycerol, and starch. Overall, the observed RhB rejection is best interpreted as the combined result (Figure 4d).
3.2.3.1 Effect of competing species on RhB rejection
In real water (containing competing NOM), all membranes showed improved RhB rejection compared to deionized water, with Starch (starch only) achieving the highest real water rejection (48.6%). This was attributed to hydrogen bonding between its abundant O-H groups and NOM, together with pore constriction and electrostatic attraction between cationic RhB and anionic NOM (Bremer and Krämer, 2026). After the membranes were fouled by real water components, RhB rejection increased dramatically for all membranes, reaching 45%–69%, far exceeding both DI water and real water values. PEG/Gly/Starch (all additives) showed the largest net gain (10.9% 69.4%, a 58.5% increase), while the PEG membrane achieved the highest absolute rejection after fouling (69.0%). This is fundamentally different from CIP rejection, which generally declined after fouling due to competition for active sites and pore blockage. The contrasting behavior is explained by RhB’s cationic charge and larger molecular size (479 g/mol, ∼1.5–1.8 nm), which creates a strong electrostatic attraction to the anionic NOM fouling layer and makes RhB susceptible to physical entrapment within the accumulated organic matrix. In contrast, CIP’s zwitterionic nature (no net charge) and smaller size (331 g/mol, 1.0–1.3 nm) allow it to bypass or diffuse through the NOM layer. These results demonstrate that membrane fouling by NOM is not universally detrimental. For cationic contaminants like RhB, the formation of an anionic fouling layer significantly enhances rejection, suggesting that real water applications may benefit from NOM accumulation when targeting positively charged pollutants (Nalawade et al., 2015). Although NOM fouling enhanced RhB rejection, it also reduced permeability as indicated in the fouling studies, indicating a trade-off between improved contaminant retention and increased hydraulic resistance.
3.2.4 Filtration of lake water samples using the fabricated membranes
Figure 5, shows the contour FEEM images of the lake water (Figure 5a) and the permeate collected after filtration with the membranes (Figures 5b–g). The rejection of NOM (Figure 5h) follows the well-established permeability–selectivity trade-off, but with notable deviations. Membranes PEG/Gly and PEG/Gly/Starch confirm the trade-off: their high flux in Figure 2d (648 and 667 L/m2h at 3 bar) is accompanied by only moderate rejection (53% average), as large pores and open structures allow solutes to pass through. PEG achieves high flux (467 L/m2h) and high rejection (60% average) due to its unique structure: an extremely thin skin with very small pores (2.2 nm) from PEG leaching, combined with massive macrovoids in the sub-layer that reduce hydraulic resistance. Based on this study, starch-modified membranes achieved the highest overall rejection (67% average) while having a relatively low flux as compared to other modified membranes (257 L/m2h). This performance is attributed to starch’s unique properties: (i) a high density of surface hydroxyl groups (confirmed by Figure 1b) that form hydrogen bonds with polar organic contaminants, particularly tyrosine-like and tryptophan-like substances; (ii) a thin, highly hydrophilic skin (contact angle 57.5°) that minimizes resistance to water flow; and (iii) a sponge-like sub-layer with shorter macrovoids (as confirmed by SEM images in Figure 1c) that increases tortuosity and provides additional adsorption sites without dramatically reducing permeability. The Starch membrane’s ability to reject both small (tyrosine-like, tryptophan-like) and large (fulvic-like, humic-like) contaminants through a combination of hydrogen bonding and size exclusion makes it the most effective membrane for real water treatment among the formulations tested (Zomorodian et al., 2018; Al-Mosawi et al., 2023).
FIGURE 5
3.2.5 Fouling tests
The fouling behavior of membranes was evaluated using two complementary approaches: (i) fouling parameters (FRR, Rt, Rr, Rir) using BSA as a model protein foulant (Figure 6a), and (ii) time-course flux decline during real water filtration using a crossflow filtration system (Figure 6b) (containing NOM and organic contaminants). BSA is widely used in the literature as a representative of a major foulant class (proteins) because its structure, mimics that of the key component of extracellular polymeric substances (EPS) and soluble microbial products (SMP), which are major foulants in bioreactors [66]. These studies revealed fundamental relationships among membrane structure, surface chemistry, and fouling resistance that are distinct from those governing rejection performance. The pristine PES exhibited the highest real water flux decline (48.5% at 180 min) with poor recovery (FRR 35.1%) and high irreversible fouling (Rir 64.9%), confirming that the unmodified hydrophobic surface (69°) promotes strong foulant adhesion without effective cleanability. Gly exhibited the best overall antifouling performance: slowest real water flux decline (41.7% at 180 min), lowest total BSA fouling (Rt 63.5%), highest flux recovery (FRR 62.2%), and low irreversible fouling (Rir 37.8%), attributed to glycerol’s hydration layer repelling both NOM and protein foulants (Hassouna et al., 2025; Zhang et al., 2024). PEG membrane exhibited a paradoxical behavior: the lowest operational flux decline in real water (20.5% at 180 min) but the worst irreversible fouling in BSA studies (Rir 70.5%) and lowest FRR (29.5%). This is explained by its very small pores (2.2 nm): NOM and BSA cause permanent pore blockage that minimally reduces flux but cannot be reversed, demonstrating that size-exclusion rejection inherently leads to irreversible fouling. The Starch membrane exhibited substantial real water flux decline (35.3% at 180 min) and high total BSA fouling (Rt 89.2%) but balanced reversible/irreversible fouling (Rr 39.2%, Rir 50.0%), consistent with its hydrogen-bonding-based rejection: strong interactions with foulants cause accumulation, but these interactions are sufficiently reversible for physical cleaning [67,68]. The PEG/Gly membrane showed the highest total BSA fouling (Rt 92.6%) and moderate real water decline (27.1% at 180 min), attributed to its large pores (7.6 nm) allowing deep foulant penetration, with moderate cleanability (FRR 43.6%). PEG/Gly/Starch (all additives) exhibited the highest reversible BSA fouling (Rr 51.2%) and second-highest FRR (59.3%), demonstrating that the irregular macrovoid structure resulting from combining all three additives creates a surface where foulants attach more loosely rather than permanently, enhancing cleanability despite moderate rejection [69]. The observed relationships between permeate flux, rejection, and fouling reversibility were governed by pore size, surface chemistry, and the dominant separation mechanism. A permeability–selectivity trade-off was evident, with PEG/Gly exhibiting the highest flux but moderate rejection, whereas Starch achieved the highest rejection at moderate flux. Fouling behavior depended on the rejection mechanism: size exclusion in PEG resulted in severe irreversible pore blocking, hydrogen bonding in Starch membrane produced balanced and more reversible fouling, and the hydration layer in Gly provided superior flux recovery through foulant repulsion. PEG/Gly/Starch exhibited the best cleanability due to weaker foulant adhesion but only moderate rejection. Overall, none of the membranes simultaneously optimized flux, rejection, and fouling resistance, highlighting the need to select membranes according to application-specific priorities.
FIGURE 6
3.2.5.1 Antimicrobial properties of the fabricated membranes
The antibacterial activity results against Staphylococcus aureus showed small zones of inhibition for Gly (6.18 mm) and PEG/Gly (6.92 mm) membranes, whereas no antimicrobial activity was noted on the other membranes (Figure 6c). The small inhibition zones observed may be attributed to the presence of residual glycerol that remains attached to the membrane after thorough post-fabrication membrane washing. The presence of glycerol-related functional groups in the modified membrane was supported by the FTIR results (Figure 1b). Residual glycerol may have been retained through interactions with the polymer matrix and physical entrapment within the membrane structure, and its possible release into the surrounding medium may have contributed to the observed inhibition. Glycerol may also exert antimicrobial effects through changes in local water activity and osmotic conditions, which may cause osmotic stress on Gram-positive bacteria such as S. aureus [70,71]. The possible contribution of glycerol leaching to the observed inhibition cannot be excluded. The absence of activity in the PEG/Gly/Starch membrane suggests that the presence of starch may hinder glycerol surface enrichment, reducing the effective surface concentration of glycerol available for antibacterial action. The starch membrane similarly showed no activity, consistent with reports in the literature that starch-based materials require functional additives (e.g., ZnO nanoparticles, essential oils) to exhibit antibacterial properties [72]. The presence of glycerol in the Gly and PEG/Gly may provide a mild antibacterial benefit for applications where biofouling resistance is desirable.
3.2.5.2 Bacterial surface colonization of the fabricated membranes
The resistance of the fabricated membranes to bacterial surface colonization was evaluated by quantifying viable S aureus cells recovered from the membrane surfaces after 1, 6, and 24 h of exposure. The results in Table 2 demonstrated a clear membrane-dependent difference in the number of viable bacteria associated with the membrane surfaces. The viable bacterial counts recovered from the membrane surfaces revealed clear differences in resistance to bacterial adhesion and colonization. Compared with pristine PES, all modified membranes showed lower viable bacterial counts after 24 h, confirming that additive incorporation generally reduced bacterial accumulation on the membrane surface. Pristine PES exhibited the highest colonization 1.12 × 107 CFU/cm2, whereas the Gly and PEG/Gly membranes showed the lowest viable counts 1.6 × 106 and 2.35 × 106 CFU/cm2, respectively. The superior performance of these two membranes, both containing glycerol, suggests that glycerol contributed favorably to resistance against bacterial surface colonization. Glycerol contains multiple hydroxyl groups that increase surface affinity for water and may promote the formation of a hydration layer, thereby reducing direct bacteria–membrane interactions. However, bacterial adhesion is governed by multiple surface properties. Roughness and surface topography can increase bacterial retention by providing additional contact area and protected attachment sites, while hydrophilic functional groups can reduce adhesion by weakening hydrophobic bacteria–surface interactions. The relatively high bacterial accumulation on the PEG membrane, despite its hydrophilic modification, shows that hydrophilicity alone was insufficient to prevent long-term colonization.
TABLE 2
| Membrane | 1 h CFU/cm2 | 6 h CFU/cm2 | 24 h CFU/cm2 |
|---|---|---|---|
| PES | 4.00 × 104 | 1.80 × 106 | 1.12 × 107 |
| Gly | not detected | 2.00 × 104 | 1.60 × 106 |
| PEG | not detected | 1.20 × 105 | 5.75 × 106 |
| Starch | not detected | 6.00 × 104 | 3.70 × 106 |
| PEG/Gly | not detected | 3.00 × 104 | 2.35 × 106 |
| PEG/Gly/Starch | not detected | 8.00 × 104 | 2.95 × 106 |
Viable Staphylococcus aureus adhesion on the surfaces of pristine and additive-modified PES membranes after 1, 6, and 24 h of exposure.
4 Conclusion
This study demonstrates that hydrophilic additive modification of PES membranes is an effective strategy for tuning membrane structure and performance, but the choice of additive and the decision to combine additives must be strategically aligned with the target application. Starch-modified membranes achieved the highest rejection of CIP (21.5%), RhB (22.9%), and NOM (67%), while glycerol provided the best antifouling performance (FRR = 62.2%). PEG/glycerol produced the highest water permeability (1238 LMH), but with lower contaminant rejection. The ternary PEG/glycerol/starch formulation did not provide an overall performance advantage under the conditions investigated. Furthermore, NOM fouling affected contaminant rejection differently, increasing RhB rejection while generally reducing CIP rejection. Overall, the findings demonstrate that hydrophilic additive selection should be based on the intended treatment objective, with different formulations offering advantages in contaminant removal, permeability, or fouling resistance.
Statements
Data availability statement
The raw data supporting the conclusions of this article will be made available by the authors, without undue reservation.
Author contributions
NP: Data curation, Investigation, Methodology, Writing – original draft. AM: Data curation, Formal Analysis, Investigation, Methodology, Writing – review and editing. MM: Formal Analysis, Investigation, Methodology, Writing – review and editing. BM: Writing – review and editing. TN: Writing – review and editing. ST: Conceptualization, Data curation, Formal Analysis, Investigation, Methodology, Supervision, Validation, Writing – original draft, Writing – review and editing.
Funding
The author(s) declared that financial support was received for this work and/or its publication. This research was funded by the Institute for Nanotechnology and Water Sustainability (iNanoWS) at the College of Science, Engineering and Technology (CSET), University of South Africa. This work is based on the research supported in part by the National Research Foundation of South Africa NRF-Thuthuka-Post-PhD Track (Reference/Grant Number: TTK23042697589).
Acknowledgments
The authors greatly acknowledge the College of Agriculture and Environmental Sciences (CAES) at the University of South Africa (UNISA) for the use of the laboratories for carrying out all the microbiology experiments.
Conflict of interest
The author(s) declared that this work was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.
Generative AI statement
The author(s) declared that generative AI was used in the creation of this manuscript. The authors used AI partially in generating the proposed mechanisms of action, AI was used together with Canva, Biorender as well as PowerPoint.
Any alternative text (alt text) provided alongside figures in this article has been generated by Frontiers with the support of artificial intelligence and reasonable efforts have been made to ensure accuracy, including review by the authors wherever possible. If you identify any issues, please contact us.
Publisher’s note
All claims expressed in this article are solely those of the authors and do not necessarily represent those of their affiliated organizations, or those of the publisher, the editors and the reviewers. Any product that may be evaluated in this article, or claim that may be made by its manufacturer, is not guaranteed or endorsed by the publisher.
References
1
AdeniyiA.OdoG. O.Gonzalez-OrtizD.Pochat-BohatierC.MbakopS.OnyangoM. S. (2023). A comparison of the effect of cellulose nanocrystals (CNCs) and polyethylene glycol (PEG) as additives in ultrafiltration membranes (PES-UF): characterization and performance. Polym. (Basel)15, 2636. 10.3390/polym15122636
2
AfzalM. Z.KhanS. A.SongC.IrfanM. I.WangS. G. (2024). Removal of ciprofloxacin via enhancing hydrophilicity of membranes using biochar. Appl. Water Sci.14, 195. 10.1007/s13201-024-02270-8
3
Al-MosawiR. M.JasimH. A.HaddadA. (2023). Study of the antibacterial effects of the starch-based zinc oxide nanoparticles on methicillin resistance Staphylococcus aureus isolates from different clinical specimens of patients from basrah. Iraq. AIMS Microbiol.9, 90–107. 10.3934/microbiol.2023006
4
Al-ShaeliM.Al-JubooriR. A.WangH.LadewigB.AlsalhyQ. F.ZhangJ. (2026). Improving fouling resistance of polyvinylidene fluoride membrane with mono-hydroxyl poly(dimethylsiloxane) (PDMS-OH) grafted silica nanoparticles. Chem. Eng. J. Adv.25, 100991. 10.1016/j.ceja.2025.100991
5
AlamM. N. E.DeowanS. A.EftyS. S.ChowdhuryF.Haque MilonA.NurnabiM. (2024). Fabrication and performance evaluation of polyethersulfone membranes with varying compositions of polyvinylpyrrolidone and polyethylene glycol for textile wastewater treatment using MBR. Heliyon10, e36215. 10.1016/j.heliyon.2024.e36215
6
AngM.MacniC. R. M.CaparangaA. R.HuangS. H.TsaiH. A.LeeK. R.et al (2020). Mitigating the fouling of mixed-matrix cellulose acetate membranes for oil–water separation through modification with polydopamine particles. Chem. Eng. Res. Des.159, 195–204. 10.1016/j.cherd.2020.04.015
7
ArahmanN.Umar BarambuN.BiladM. R.MulyatiS.RosnellyC. M.ApriliaS. (2026). Strategies for the development of antifouling membranes for liquid filtration: a review. J. Hazard. Mater. Adv.21, 100958. 10.1016/j.hazadv.2025.100958
8
BremerE.KrämerR. (2026). Responses of Microorganisms to Osmotic Stress. 10.1146/annurev-micro-020518-115504
9
ChakachakaV. M.MahlanguO. T.TshanganaC. S.MambaB. B.MulejaA. A. (2023). Highly adhesive CoFe2O4 nanoengineered PES membranes for salts and naproxen removal and antimicrobial activities. J. Memb. Sci.676, 121612. 10.1016/j.memsci.2023.121612
10
EnyohC. E.WangQ. (2024). Adsorption of ciprofloxacin from aqueous solution by plastic-based adsorbents: a review. Int. J. Environ. Anal. Chem.104, 4557–4577. 10.1080/03067319.2022.2106432
11
FoorginezhadS.ZerafatM. M.IsmailA. F.GohP. S. (2025). Emerging membrane technologies for sustainable water treatment: a review on recent advances. Environ. Sci. Adv.4, 530–570. 10.1039/d4va00378k
12
GayatriR.FizalA. N. S.YuliwatiE.HossainM. S.JaafarJ.ZulkifliM.et al (2023). Preparation and characterization of PVDF–TiO2 mixed-matrix membrane with PVP and PEG as pore-forming agents for BSA rejection. Nanomaterials13, 1023. 10.3390/nano13061023
13
GongB.ChenW.QianC.SitP. H. L.LiuX. W.YuH. Q. (2023). Contribution of proteins to ceramic membrane fouling at the early stage of membrane filtration. Sep. Purif. Technol.312, 123450. 10.1016/j.seppur.2023.123450
14
GumbiN. N. (2019). Carbon Nanotube Membranes for Brackish Groundwater Desalination and Removal of Organic Micropollutants from Water. University of South Africa.
15
Hainiza Abd-RazakN.Zairossani andM. N.ChewY. M. J.BirdM. R. (2020). Fouling Analysis and the Recovery of Phytosterols from Orange Juice Using Regenerated Cellulose Ultrafiltration Membranes. 10.1007/s11947-020-02541-7/Published
16
HassounaM.NasserN.SalemN.AmerR.KandilS. H.NadyN. (2025). Inhibition of bacterial attachment to polyethersulfone membranes using aminophenol compounds in static and continuous flow systems. Sci. Rep.15, 30723. 10.1038/s41598-025-15558-9
17
HawaM. S.AbdullahH. Z.HarunZ. (2013). Jurnal teknologi membrane performance: TiO 2 nanoparticles coated on polysulfone (PSf) ultrafiltration membrane surfaces.
18
HeH.WenJ.ZhaoQ.KeG.YangH. (2023). The adsorption activity and mechanism of common tourmalines for typical anionic and cationic dyes. Chem. Phys.571, 111938. 10.1016/j.chemphys.2023.111938
19
HorkáM.VykydalováM.RůžičkaF.ŠalplachtaJ.HoláV.DvořáčkováM.et al (2014). CIEF separation, UV detection, and quantification of ampholytic antibiotics and bacteria from different matrices. Anal. Bioanal. Chem.406, 6285–6296. 10.1007/s00216-014-8053-8
20
Ignaciode LeonP. A. A.ZharovI. (2011). Size-selective molecular transport through silica colloidal nanopores. Chem. Commun.47, 553–555. 10.1039/c0cc02101f
21
IlomäkiJ. (2023). Effect of organic matrix on the adsorption of selected antibiotics and antiretroviral drugs from drinking water onto activated carbon.
22
Jason KwongM. L. G. (2017). Kucers’ the Use of Antibiotics. 7th ed.CRC Press. 10.1201/9781498747967
23
KaszásN.BozóT.BudaiM.GrófP. (2013). Ciprofloxacin encapsulation into giant unilamellar vesicles: membrane binding and release. J. Pharm. Sci.102, 694–705. 10.1002/jps.23410
24
KedangY. I.PriyanggaA.AtmajaL.SantosoM. (2022). Characteristics and performance studies of a composite polymer electrolyte membrane based on chitosan/glycerol-sulfosuccinic acid modified montmorillonite clay. RSC Adv.12, 30742–30753. 10.1039/d2ra04560e
25
KooI. K.ChongM. N.GohK. B. (2025). Gradient or no gradient: spatial hydrostatic pressure distributions in bilayer thin-film composite membranes. J. Memb. Sci.727, 124023. 10.1016/j.memsci.2025.124023
26
KouhestaniF.TorangiM. A.MotavalizadehkakhkyA.KarazhyanR.ZhianiR. (2019). Enhancement strategy of polyethersulfone (pes) membrane by introducing pluronic f127/graphene oxide and phytic acid/graphene oxide blended additives: preparation, characterization and wastewater filtration assessment. Desalination Water Treat.171, 44–56. 10.5004/dwt.2019.24769
27
KuśmierekK.FronczykJ.ŚwiątkowskiA. (2023). Adsorptive removal of rhodamine B dye from aqueous solutions using mineral materials as low-cost adsorbents. Water Air Soil Pollut.234, 531. 10.1007/s11270-023-06511-5
28
LagiewkaJ.WittK.GierszewskaM.ZawieruchaI. (2024). Selective removal of organic dyes via polymer inclusion membrane containing a perbenzylated β-cyclodextrin derivative. J. Water Process Eng.68, 106306. 10.1016/j.jwpe.2024.106306
29
LaliaB. S.KochkodanV.HashaikehR.HilalN. (2013). A review on membrane fabrication: structure, properties and performance relationship. Desalination326, 77–95. 10.1016/j.desal.2013.06.016
30
LiuB.YinJ.WuJ.ChengX.YangK.LiG.et al (2022). Effect of UV/ClO2 pretreatment on controlling ultrafiltration membrane fouling of different natural organic matter (NOM) fractions. J. Water Process Eng.49, 103156. 10.1016/j.jwpe.2022.103156
31
MaY.ShiF.MaJ.WuM.ZhangJ.GaoC. (2011). Effect of PEG additive on the morphology and performance of polysulfone ultrafiltration membranes. Desalination272, 51–58. 10.1016/j.desal.2010.12.054
32
MabasoN. S. N.TshanganaC. S.NkambuleT. T. I.MulejaA. A. (2026). Photocatalytic removal of ciprofloxacin in drinking water treatment plant process using nanocomposite BN/TiO2. Int. J. Environ. Sci. Technol.23, 411. 10.1007/s13762-026-07189-y
33
MahlanguO. T.MotsaM. M.HaiF. I.MambaB. B. (2023). Role of membrane–solute affinity interactions in carbamazepine rejection and resistance to organic fouling by nano-engineered UF/PES membranes. Membr. (Basel)13, 744. 10.3390/membranes13080744
34
MambaP. P.MsagatiT. A. M.MambaB. B.MotsaM. M.NkambuleT. T. I. (2024). The removal of pathogenic bacteria and dissolved organic matter from freshwater using microporous membranes: insights into biofilm formation and fouling reversibility. Biofouling40, 245–261. 10.1080/08927014.2024.2339438
35
MamtoraD.KuradaK. V. (2025). Morphology-based prediction of permeability of asymmetric polymeric membranes. Polym. Eng. Sci.65, 4131–4142. 10.1002/pen.27280
36
ManawiY.KochkodanV.MahmoudiE.JohnsonD. J.MohammadA. W.AtiehM. A. (2017). Characterization and separation performance of a novel polyethersulfone membrane blended with acacia gum. Sci. Rep.7, 15831. 10.1038/s41598-017-14735-9
37
MantelT.JackiE.ErnstM. (2021). Electrosorptive removal of organic water constituents by positively charged electrically conductive UF membranes. Water Res.201, 117318. 10.1016/j.watres.2021.117318
38
MatebeseF.RasealaM. J.MotloutsiM. L.MoutloaliR. M. (2025). Fabrication and characterization of PAA-g-PES polymers and resultant membranes: combating fouling through the introduction of hydrophilic PAA brushes. ACS Omega10, 22397–22411. 10.1021/acsomega.4c05443
39
MudauF. H.MahlanguO. T.De KockL.-A.MotsaM. M. (2026). Poly (methacrylic acid)/starch incorporated low-pressure polyethersulfone (ultrafiltration) membranes for slaughterhouse wastewater treatment intended for reuse. Int. J. Environ. Sci. Technol.23, 243. 10.1007/s13762-026-07061-z
40
NalawadeT.BhatK.SumaHPS. (2015). Bactericidal activity of propylene glycol, glycerine, polyethylene glycol 400, and polyethylene glycol 1000 against selected microorganisms. J. Int. Soc. Prev. Community Dent.5, 114–119. 10.4103/2231-0762.155736
41
NhlengethwaS. T.TshanganaC. S.MambaB. B.MulejaA. A. (2024). The application of TiO2/ZrO2-Modified nanocomposite PES membrane for improved permeability of textile dye in water. Membr. (Basel)14, 222. 10.3390/membranes14100222
42
NhlengethwaS. T.TshanganaC. S.GlassS.DenisonS.YanL.NkambuleT. T. I.et al (2025). Superhydrophilic TiO2/WO2.72 nanocomposites boost PES membranes performance for natural spring water decontamination. Adv. Mater Interfaces12, e00598. 10.1002/admi.202500598
43
NilssenE.WormaldP. J.OliverS. (1996). Glycerol and ichthammol: medicinal solution or mythical potion?J. Laryngology Otology110, 319–321. 10.1017/s0022215100133547
44
PaluchM.OstrowskaJ.TyńskiP.SadurskiW.KonkolM. (2022). Structural and thermal properties of starch plasticized with glycerol/urea mixture. J. Polym. Environ.30, 728–740. 10.1007/s10924-021-02235-x
45
PanZ.LeiY.YanT.ZhengF.LiaoY.ZhanJ.et al (2025). Molecular manipulation of polyamide nanostructures reconciles the permeance-selectivity threshold for precise ion separation. Nat. Commun.16, 7171. 10.1038/s41467-025-62376-8
46
PengS.WangZ.QiF.LiC.XuM.SongZ.et al (2022). Novel insights into the interaction reactive components and synergistic fouling mechanisms of ultrafiltration by natural organic matter fractions and kaolin. Environ. Res.212, 113285. 10.1016/j.envres.2022.113285
47
PhillipN.MulejaA. A.MotsaM. M.MambaB. B.NkambuleT. T. I.TshanganaC. S. (2026). Membrane biofouling: current understanding and future Perspectives- an overview. Curr. Microbiol.83, 299. 10.1007/s00284-026-04882-6
48
QalyoubiL.Al-OthmanA.Al-AshehS. (2022). Removal of ciprofloxacin antibiotic pollutants from wastewater using nano-composite adsorptive membranes. Environ. Res.215, 114182. 10.1016/j.envres.2022.114182
49
SaediS.MadaeniS. S.SeidiF.ShamsabadiA. A.LakiS. (2013). Synthesis and application of a novel amino-starch derivative as a new polymeric additive for fixed facilitated transport of carbon dioxide through an asymmetric polyethersulfone (PES) membrane. Int. J. Greenh. Gas Control19, 126–137. 10.1016/j.ijggc.2013.06.019
50
SałacińskaA.SienkiewiczP.SzymańskiK.MoziaS. (2024). Polyethersulfone mixed matrix membranes modified with pore formers and Ag-titanate nanotubes: physicochemical characteristics and (bio)fouling study. Environ. Sci. Pollut. Res.31, 63876–63894. 10.1007/s11356-024-35461-6
51
SaraviaF.FrimmelF. H. (2008). Role of NOM in the performance of adsorption-membrane hybrid systems applied for the removal of pharmaceuticals. Desalination224, 168–171. 10.1016/j.desal.2007.02.089
52
Shirzadeh-GharachehA.Rahbari-SisakhtM. (2016). Polyvinylidene fluoride hollow fiber mixed matrix membrane contactor incorporating modified ZSM-5 zeolite for carbon dioxide absorption. RSC Adv.6, 78865–78874. 10.1039/c6ra15375e
53
SuJ. F.HiepN. T. (2025). Fabrication of glycerol-engineered asymmetric polyethersulfone ultrafiltration membranes with enhanced flux and separation performance. J. Taiwan Inst. Chem. Eng.184, 106345. 10.1016/j.jtice.2025.106345
54
TripathiB. P.DubeyN. C.StammM. (2014). Polyethylene glycol cross-linked sulfonated polyethersulfone based filtration membranes with improved antifouling tendency. J. Memb. Sci.453, 263–274. 10.1016/j.memsci.2013.11.007
55
TshanganaS. C. (2022). Graphene Oxide Quantum Dots-based Nanocomposites for Wastewater Treatment. University of South Africa.
56
TshanganaC.MulejaA. (2024). Graphene oxide quantum dots membrane: a hybrid filtration-advanced technology system to enhance process of wastewater reclamation. Chem. Pap.78, 1317–1333. 10.1007/s11696-023-03187-3
57
TsoleleR.ArotibaO. A.MalingaS. P. (2025). Improving selectivity and antifouling properties of a PES hollow fibre membrane with a photo-enzyme for the removal of ciprofloxacin and sulfamethoxazole. Environ. Technol. (United Kingdom)46, 453–476. 10.1080/09593330.2024.2360231
58
WangH.WangX.YuY.MambaB. B.JiangX.YangX.et al (2026). Engineering self-rebound catalytic membranes for efficient high-viscosity oily wastewater purification and emerging contaminants removal. Water Res.288, 124750. 10.1016/j.watres.2025.124750
59
WenX.HeC.HaiY.MaR.SunJ.YangX.et al (2022). Fabrication of an antifouling PES ultrafiltration membrane: Via blending SPSF. RSC Adv.12, 1460–1470. 10.1039/d1ra06354e
60
YildizY.ManzakA. (2024). The effect of a hydrophilic polymer on the morphology of polymeric membranes and the retention of metals. Water Air Soil Pollut.235, 517. 10.1007/s11270-024-07324-w
61
YuH.XuR.RenJ.YuanL.CuiZ.ZhangW.et al (2026). MXene membrane with directionally functionalized channel entrances for enhanced ion selectivity and permeability. Nat. Commun.17, 6282. 10.1038/s41467-026-71889-9
62
ZazouliM. A.NasseriS.MahviA. H.GholamiM.MesdaghiniaA. R.YounesianM. (2008). Retention of Humic Acid from Water by Nanofiltration Membrane and Influence of Solution Chemistry on Membrane Performance, 5.
63
ZhangX.LiaoZ.ZhangX.RuanX.GongH.WangX.et al (2024). Hydrophilic modified PES asymmetric membrane via thermal cross-linking for artificial lung application. Sep. Purif. Technol.347, 127501. 10.1016/j.seppur.2024.127501
64
ZhaoH.HeT.YaoS.TaoL.ZhangX.WangZ.et al (2024). Improved protein removal performance of PES hollow-fiber ultrafiltration membrane with sponge-like structure. Polym. (Basel)16, 1194. 10.3390/polym16091194
65
ZomorodianK.VeisiH.MousaviS. M.AtaabadiM. S.YazdanpanahS.BagheriJ.et al (2018). Modified magnetic nanoparticles by PEG-400-immobilized ag nanoparticles (Fe3O4@PEG–Ag) as a core/shell nanocomposite and evaluation of its antimicrobial activity. Int. J. Nanomedicine13, 3965–3973. 10.2147/IJN.S161002
Summary
Keywords
dye rejection, hydrophilic additives, membrane filtration, membrane modification, natural organic matter
Citation
Phillip N, Muleja AA, Motsa MM, Mamba BB, Nkambule TTI and Tshangana SC (2026) Non-polymeric solvents as membrane additives for tailoring membrane structure and performance. Front. Environ. Chem. 7:1949697. doi: 10.3389/fenvc.2026.1949697
Received
27 July 2026
Revised
17 September 2026
Accepted
24 September 2026
Published
13 October 2026
Volume
7 - 2026
Edited by
Ajith Manayil Parambil, VSB-Technical University of Ostrava, Czechia
Reviewed by
Shounik Paul, Indian Institute of Science Education and Research Kolkata, India
Devi Sri Rajendran, SRM Institute of Science and Technology, India
Avani Alayil Veedu, Indian Institute of Technology Madras, India
Updates
Copyright
© 2026 Phillip, Muleja, Motsa, Mamba, Nkambule and Tshangana.
This is an open-access article distributed under the terms of the Creative Commons Attribution License (CC BY). The use, distribution or reproduction in other forums is permitted, provided the original author(s) and the copyright owner(s) are credited and that the original publication in this journal is cited, in accordance with accepted academic practice. No use, distribution or reproduction is permitted which does not comply with these terms.
*Correspondence: S. C. Tshangana, tshansc@unisa.ac.za
Disclaimer
All claims expressed in this article are solely those of the authors and do not necessarily represent those of their affiliated organizations, or those of the publisher, the editors and the reviewers. Any product that may be evaluated in this article or claim that may be made by its manufacturer is not guaranteed or endorsed by the publisher.