<?xml version="1.0" encoding="UTF-8"?>
<!DOCTYPE article PUBLIC "-//NLM//DTD Journal Publishing DTD v2.3 20070202//EN" "journalpublishing.dtd">
<article article-type="research-article" dtd-version="2.3" xml:lang="EN" xmlns:mml="http://www.w3.org/1998/Math/MathML" xmlns:xlink="http://www.w3.org/1999/xlink">
<front>
<journal-meta>
<journal-id journal-id-type="publisher-id">Front. Mater.</journal-id>
<journal-title>Frontiers in Materials</journal-title>
<abbrev-journal-title abbrev-type="pubmed">Front. Mater.</abbrev-journal-title>
<issn pub-type="epub">2296-8016</issn>
<publisher>
<publisher-name>Frontiers Media S.A.</publisher-name>
</publisher>
</journal-meta>
<article-meta>
<article-id pub-id-type="publisher-id">588716</article-id>
<article-id pub-id-type="doi">10.3389/fmats.2020.588716</article-id>
<article-categories>
<subj-group subj-group-type="heading">
<subject>Materials</subject>
<subj-group>
<subject>Original Research</subject>
</subj-group>
</subj-group>
</article-categories>
<title-group>
<article-title>The Influence of Si<sub>3</sub>N<sub>4w</sub> Volume Fraction on the Microstructure and Properties of Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> Composites via CVI Technique</article-title>
<alt-title alt-title-type="left-running-head">Chen et al.</alt-title>
<alt-title alt-title-type="right-running-head">Tunable Wave-Transparent Property of Si3N4w/Si3N4 Composites</alt-title>
</title-group>
<contrib-group>
<contrib contrib-type="author">
<name>
<surname>Chen</surname>
<given-names>Chao</given-names>
</name>
<xref ref-type="aff" rid="aff1">
<sup>1</sup>
</xref>
<uri xlink:href="http://loop.frontiersin.org/people/1087761/overview"/>
</contrib>
<contrib contrib-type="author" corresp="yes">
<name>
<surname>Liu</surname>
<given-names>Yongsheng</given-names>
</name>
<xref ref-type="aff" rid="aff1">
<sup>1</sup>
</xref>
<xref ref-type="aff" rid="aff2">
<sup>2</sup>
</xref>
<xref ref-type="corresp" rid="c001">&#x2a;</xref>
</contrib>
<contrib contrib-type="author">
<name>
<surname>Yue</surname>
<given-names>Wei</given-names>
</name>
<xref ref-type="aff" rid="aff1">
<sup>1</sup>
</xref>
<uri xlink:href="http://loop.frontiersin.org/people/777521/overview"/>
</contrib>
<contrib contrib-type="author">
<name>
<surname>Ye</surname>
<given-names>Fang</given-names>
</name>
<xref ref-type="aff" rid="aff1">
<sup>1</sup>
</xref>
</contrib>
<contrib contrib-type="author">
<name>
<surname>Wang</surname>
<given-names>Jing</given-names>
</name>
<xref ref-type="aff" rid="aff1">
<sup>1</sup>
</xref>
</contrib>
<contrib contrib-type="author">
<name>
<surname>Zeng</surname>
<given-names>Qingfeng</given-names>
</name>
<xref ref-type="aff" rid="aff1">
<sup>1</sup>
</xref>
</contrib>
</contrib-group>
<aff id="aff1">
<label>
<sup>1</sup>
</label>Science and Technology on Thermostructural Composite Materials Laboratory, Northwestern Polytechnical University, <addr-line>Xi&#x2019;an</addr-line>, <country>China</country>
</aff>
<aff id="aff2">
<label>
<sup>2</sup>
</label>NPU-SAS Joint Research Center of Advanced Ceramics, Northwestern Polytechnical University, <addr-line>Xi&#x2019;an</addr-line>, <country>China</country>
</aff>
<author-notes>
<fn fn-type="edited-by">
<p>
<bold>Edited by:</bold> <ext-link ext-link-type="uri" xlink:href="https://loop.frontiersin.org/people/560305/overview">Yang Bai</ext-link>, University of Oulu, Finland</p>
</fn>
<fn fn-type="edited-by">
<p>
<bold>Reviewed by:</bold> <ext-link ext-link-type="uri" xlink:href="https://loop.frontiersin.org/people/1048844/overview">Yan Zhang</ext-link>, Central South University, China</p>
<p>
<ext-link ext-link-type="uri" xlink:href="https://loop.frontiersin.org/people/353145/overview">Subhasis Roy</ext-link>, University of Calcutta, India</p>
</fn>
<corresp id="c001">&#x2a;Correspondence: Yongsheng Liu, <email>yongshengliu@nwpu.edu.cn</email>
</corresp>
<fn fn-type="other">
<p>This article was submitted to Ceramics and Glass, a section of the journal Frontiers in Materials</p>
</fn>
</author-notes>
<pub-date pub-type="epub">
<day>27</day>
<month>11</month>
<year>2020</year>
</pub-date>
<pub-date pub-type="collection">
<year>2020</year>
</pub-date>
<volume>7</volume>
<elocation-id>588716</elocation-id>
<history>
<date date-type="received">
<day>29</day>
<month>07</month>
<year>2020</year>
</date>
<date date-type="accepted">
<day>19</day>
<month>10</month>
<year>2020</year>
</date>
</history>
<permissions>
<copyright-statement>Copyright &#x00A9; 2020 Chen, Liu, Yue, Ye, Wang and Zeng</copyright-statement>
<copyright-holder>Chen, Liu, Yue, Ye, Wang and Zeng</copyright-holder>
<license xlink:href="http://creativecommons.org/licenses/by/4.0/">
<p>This is an open-access article distributed under the terms of the Creative Commons Attribution License (CC BY). The use, distribution or reproduction in other forums is permitted, provided the original author(s) and the copyright owner(s) are credited and that the original publication in this journal is cited, in accordance with accepted academic practice. No use, distribution or reproduction is permitted which does not comply with these terms.</p>
</license>
</permissions>
<abstract>
<p>Wave-transparent ceramic composites with excellent comprehensive performances are of particular significance for the development of space vehicles. In this study, Si<sub>3</sub>N<sub>4w</sub> was prepared by the gel-casting process and then combined with chemical vapor infiltration (CVI)-obtained Si<sub>3</sub>N<sub>4</sub> to yield Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> composites with five Si<sub>3</sub>N<sub>4w</sub> volume fractions. The influence of the Si<sub>3</sub>N<sub>4w</sub> volume fraction on the microstructures, mechanical properties, and dielectric characteristics of the Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> composites were all studied. The results showed that Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> composites possess A sandwich structures. Higher Si<sub>3</sub>N<sub>4w</sub> volume fractions led to less incorporated amounts of the Si<sub>3</sub>N<sub>4</sub> matrix at the same depth. The 25&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> composites integrated relatively higher Si<sub>3</sub>N<sub>4w</sub> volume fraction and load transfer ability of the matrix, leading to better flexural strengths reaching up to 41.37&#xa0;MPa. The dielectric constants of the five prepared Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> composites ranged from 2.25 to 4.0. The dielectric losses were all lower than 0.005, demonstrating the good dielectric properties of the Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> composites.</p>
</abstract>
<kwd-group>
<kwd>Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> composites</kwd>
<kwd>gel-casting</kwd>
<kwd>chemical vapor infiltration</kwd>
<kwd>dielectric properties</kwd>
<kwd>mechanical properties</kwd>
</kwd-group>
<contract-num rid="cn001">51672217</contract-num>
<contract-sponsor id="cn001">National Natural Science Foundation of China<named-content content-type="fundref-id">10.13039/501100001809</named-content>
</contract-sponsor>
<counts>
<page-count count="0"/>
</counts>
</article-meta>
</front>
<body>
<sec id="s1">
<title>Introduction</title>
<p>High-temperature wave-transparent materials are used in spacecraft radomes and antenna windows, which require good mechanical and dielectric properties, as well as high-temperature resistance. Therefore, the development of novel wave-transparent materials with elevated wave transmittance and strength is of great significance for advanced and reliable applications (<xref ref-type="bibr" rid="B14">Medding, 1996</xref>; <xref ref-type="bibr" rid="B3">Bolivar et al., 2003</xref>; <xref ref-type="bibr" rid="B2">Ashok et al., 2007</xref>; <xref ref-type="bibr" rid="B10">Kandi et al., 2014</xref>; <xref ref-type="bibr" rid="B7">Hehdari et al., 2017</xref>).</p>
<p>Si<sub>3</sub>N<sub>4</sub>-based ceramics are employed in wave-transparent materials due to their excellent comprehensive performances (<xref ref-type="bibr" rid="B1">Arakawa et al., 1991</xref>; <xref ref-type="bibr" rid="B8">Hsieh and Mizuhara, 1987</xref>; <xref ref-type="bibr" rid="B9">Hsieh, 1987</xref>; <xref ref-type="bibr" rid="B24">Zou et al., 2009</xref>). For instance, <xref ref-type="bibr" rid="B20">Xu et al. (2020)</xref> studied the influence of different sintering additives on the dielectric properties of reaction-bonded Si<sub>3</sub>N<sub>4</sub>. Their results showed that the addition of Y<sub>2</sub>O<sub>3</sub> and La<sub>2</sub>O<sub>3</sub> powders may generate Y-Si-O-N and La-Si-O-N phases, further increasing the dielectric constant and dielectric loss <xref ref-type="bibr" rid="B2">Lee et al. (2000)</xref> prepared a Si<sub>3</sub>N<sub>4</sub>w/Si<sub>3</sub>N<sub>4</sub> composite by the Gas Pressure Sintering (GPS) method. The amount of &#x3b2;-Si<sub>3</sub>N<sub>4</sub>w changed the microstructure, which changed the thermal conductivity. <xref ref-type="bibr" rid="B6">Ding et al. (2007)</xref> sintered Si<sub>3</sub>N<sub>4</sub> powders at 1,200&#x2013;1,500&#xb0;C under air to yield prepared Si<sub>3</sub>N<sub>4</sub> ceramics with a SiO<sub>2</sub> coating on the surface. The influence of sintering temperature and holding time on the oxidation degree, porosity, flexural strength, and dielectric properties were all studied. The highest flexural strength of prepared Si<sub>3</sub>N<sub>4</sub> ceramics reached 136.9&#xa0;MPa and the lowest dielectric constant was 3.1.</p>
<p>To synergistically improve the mechanical and dielectric properties, the development of silicon nitride-based wave-transparent composite materials is increasingly considered (<xref ref-type="bibr" rid="B4">Cao et al., 2013</xref>; <xref ref-type="bibr" rid="B18">Wan et al., 2016</xref>). For example, <xref ref-type="bibr" rid="B21">Yang et al. (2019)</xref> (<xref ref-type="bibr" rid="B12">Li et al., 2019</xref>) prepared unidirectional silicon nitride fiber-reinforced silica composites by monofilament winding combined with the sol-gel method. The composite prepared by sintering under an N<sub>2</sub> atmosphere showed the highest flexural strengths reaching up 210&#xa0;MPa at 1,200&#xb0;C. Besides, the flexural strength improved from 160 to 210&#xa0;MPa at 900&#xb0;C due to the release of stress in the fiber. Meanwhile, a Si<sub>3</sub>N<sub>4f</sub>/SiON/SiO<sub>2</sub> composite has been prepared by introducing a SiON interphase using the precursor transformation method. After decarbonization by annealing, the flexural strength of Si<sub>3</sub>N<sub>4f</sub>/SiON/SiO<sub>2</sub> decreased by 35% when compared to Si<sub>3</sub>N<sub>4f</sub>/SiO<sub>2</sub> but the fracture toughness improved. <xref ref-type="bibr" rid="B5">Cheng et al. (2019)</xref> assembled porous Si<sub>3</sub>N<sub>4</sub>/Si<sub>3</sub>N<sub>4</sub> composites by 3D printing combined with the chemical vapor infiltration (CVI) method. The increase in CVI processing to 12&#xa0;h led to a decline in the porosity from 68.65 to 12.07. Meanwhile, the dielectric constant increased from 1.72 to 3.6 but the dielectric loss was always lower than 0.01. Since 2003, polysilazane has been used as a precursor in combination with the polymer infiltration pyrolysis process to prepare SiO<sub>2f</sub>/Si<sub>3</sub>N<sub>4</sub> with good mechanical and high-temperature dielectric properties (<xref ref-type="bibr" rid="B15">Qi et al., 2005a</xref>; <xref ref-type="bibr" rid="B16">Qi et al., 2005b</xref>; <xref ref-type="bibr" rid="B17">Qi et al., 2005c</xref>).</p>
<p>However, extremely high or low volume fractions of reinforcement in the ceramic matrix composites should lead to the declined mechanical properties of the resulting composite materials. Besides, different reinforcement volume fractions should result in variable contents and distributions of reinforcement, as well as various matrices and pores, further influencing the dielectric properties of the composites. Therefore, clarifying the influencing rules of the reinforcement volume fractions on the mechanical and dielectric properties of ceramic matrix composites is highly desirable for advanced applications.</p>
<p>
<xref ref-type="bibr" rid="B13">Li et al. (2020)</xref> prepared zirconia fiber hybrid alumina fiber/boron phenolic (ZA/BPF) composites with fiber volume fractions of 5, 10, 15, 25, and 30&#xa0;vol%. The microscopic results showed that extremely low and high reinforcement volume fractions resulted in weak bonding between the matrix and fiber. At a fiber volume fraction of 25%, the maximum flexural strengths of the composites reached 48.86&#xa0;MPa. Using the hot-pressing sintering method, <xref ref-type="bibr" rid="B19">Xu et al. (1994)</xref> prepared SiC<sub>f</sub>/Si<sub>3</sub>N<sub>4</sub> with a fiber volume fraction of 14, 29, and 55&#xa0;vol%. Their data suggested that the flexural strength of the composites first increased with the fiber volume fraction and then decreased. The reason for the reduction in strength was related to the fiber damage caused by its contact during the hot-pressing process of high volume fraction composites.</p>
<p>In this work, five preforms of Si<sub>3</sub>N<sub>4w</sub> volume fractions (5, 15, 25, 35, and 45&#xa0;vol%) were prepared by the gel-casting process. Different volume fractions of the Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> composites were then obtained by introducing a Si<sub>3</sub>N<sub>4</sub> matrix through the CVI Si<sub>3</sub>N<sub>4</sub> process. The effects of whisker volume fractions on the microstructures, mechanical properties, and dielectric characteristics of the Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> composites were all studied. The results suggested that the 25&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> possessed the highest comprehensive performances.</p>
</sec>
<sec id="s2">
<title>Experiment</title>
<sec id="s2-1">
<title>Raw Materials</title>
<p>Water-based gel casting was used to prepare the Si<sub>3</sub>N<sub>4w</sub> preforms with different volume fractions. Firstly, Si<sub>3</sub>N<sub>4</sub>w was used to configure the Si<sub>3</sub>N<sub>4</sub>w slurry, then PMMA was added after ball milling for 4&#xa0;h. Subsequently, the slurry was heated at 70&#xb0;C to cure for 2&#xa0;h. After drying, it was discharged at 400&#xb0;C to create the Si<sub>3</sub>N<sub>4</sub>w performs. Si<sub>3</sub>N<sub>4w</sub> with a length of 4&#x2013;12&#xa0;&#x3bc;m (average 8&#xa0;&#x3bc;m), diameter of 0.8&#x2013;1.2&#xa0;&#x3bc;m (average 1&#xa0;&#x3bc;m), and average aspect ratio of 8:1 was prepared in our laboratory. Polymethyl methacrylate (PMMA; Wuhan Yuancheng Technology Development Co., Ltd.) was employed as the pore former, acrylamide (Tianjin Comeo Chemical Reagent Co., Ltd.) as a monomer, and methylenebisacrylamide (MACLIN) as a crosslinking agent.</p>
<p>SiCl<sub>4</sub>-NH<sub>3</sub>-H<sub>2</sub>-Ar was utilized as a gas source system for the preparation of the Si<sub>3</sub>N<sub>4</sub> matrix by CVI, SiCl<sub>4</sub> as a source of Si element, and H<sub>2</sub> as a carrier and dilution gas. In this process, H<sub>2</sub> was passed through the liquid SiCl<sub>4</sub> to take the saturated SiCl<sub>4</sub> vapor into the reaction furnace in actual production. NH<sub>3</sub> was employed as a source of N element and Ar as a dilution gas. SiCl<sub>4</sub>, H<sub>2,</sub> and Ar with a purity of 99.999&#xa0;vol% were all obtained from the Sichuan Messer Gas Products Co., Ltd., Xi&#x2019;an branch. NH<sub>3</sub> (purity 99.99&#xa0;vol%) was purchased from the Beijing Marty Technology Co., Ltd.</p>
</sec>
<sec id="s2-2">
<title>Experimental Process</title>
<p>Sizing agents with Si<sub>3</sub>N<sub>4w</sub> volume fractions of 5, 15, 25, 35, and 45&#xa0;vol% were prepared to yield preforms with Si<sub>3</sub>N<sub>4w</sub> volume fractions of 10, 20, 30, 40, and 50&#xa0;vol% after solidification and decarbonization processes, respectively. To prevent over-shrinkage during the preparation of preforms at low volume fractions of Si<sub>3</sub>N<sub>4w</sub>, PMMA was added as a pore former in the sizing agent.</p>
<p>Using the CVI Si<sub>3</sub>N<sub>4</sub> process, Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> composites with five-volume fractions of Si<sub>3</sub>N<sub>4w</sub> preforms were prepared and placed in the graphite mold. The CVI process are described in detail in literature (<xref ref-type="bibr" rid="B22">Zhou et al., 2019a</xref>). The preparation process was divided into six periods, each consisting of 60&#xa0;h. For the convenience of subsequent expressions, the abbreviation 15&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> represented the composite prepared using the size agent with 15&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>, the same as the other composites. The influences of volume fractions of Si<sub>3</sub>N<sub>4w</sub> on the microstructures, mechanical properties, and dielectric characteristics of Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> were all studied.</p>
</sec>
<sec id="s2-3">
<title>Characterization</title>
<p>The density and porosity of each sample were tested by the Archimedes drainage method using AG204 electronic analytic balance by Mettler Toledo (accuracy 0.0001&#xa0;g). The microstructures were viewed by a Helios G4 CX focused ion-electron double beam electron microscope (FEI). The flexural strength and fracture toughness values at loading speeds of 0.5 and 0.05&#xa0;mm/min were obtained by the SANS CMT4304 electronic universal testing machine. The dielectric properties were tested by a vector network analyzer (MS4644A, produced by Anritsu, Japan). The experiments were performed at a standard dielectric sample size of 22.86&#xa0;mm &#xd7; 10.16&#xa0;mm &#xd7; <italic>h</italic>&#xa0;mm and a testing frequency band of 8.2&#x2013;12.4&#xa0;GHz.</p>
</sec>
</sec>
<sec sec-type="results|discussion" id="s3">
<title>Results and Discussion</title>
<sec id="s3-1">
<title>Microstructure</title>
<p>The morphology of the Si<sub>3</sub>N<sub>4w</sub> preform before decarbonization is shown in <xref ref-type="fig" rid="F1">Figure 1</xref>. The macro photo of the Si<sub>3</sub>N<sub>4w</sub> preform before decarbonization displayed a polymer matrix composite of certain strength and hardness, and it can be transferred without being destroyed after forming (<xref ref-type="fig" rid="F1">Figures 1A</xref>). The smooth and flat surface revealed the advantages of the gel-casting in terms of near net-size forming. The high magnification SEM photo in <xref ref-type="fig" rid="F1">Figures 1B</xref> exhibits the intact structures of Si<sub>3</sub>N<sub>4w</sub> and PMMA. The PMMA sphere with a diameter of approximately 5&#xa0;&#x3bc;m could support the whisker structure. The low magnification SEM photo in <xref ref-type="fig" rid="F1">Figures 1C</xref> reveals evenly dispersed dSi<sub>3</sub>N<sub>4w</sub> and PMMA, beneficial to the formation of connected pores after decarbonization.</p>
<fig id="F1" position="float">
<label>FIGURE 1</label>
<caption>
<p>Morphology of the Si<sub>3</sub>N<sub>4w</sub> preform before decarbonization: <bold>(A)</bold> macro photo; <bold>(B)</bold> high magnification SEM photo of section; <bold>(C)</bold> low magnification SEM photo of section.</p>
</caption>
<graphic xlink:href="fmats-07-588716-g001.tif"/>
</fig>
<p>The morphology of the Si<sub>3</sub>N<sub>4w</sub> preform after decarbonization is shown in <xref ref-type="fig" rid="F2">Figure 2</xref>. The preform kept a perfectly consistent appearance during the decarbonization process (<xref ref-type="fig" rid="F2">Figures 2A</xref>). In the SEM photo of <xref ref-type="fig" rid="F2">Figures 2B</xref>, the shape of Si<sub>3</sub>N<sub>4w</sub> was completely preserved and the PMMA spheres were fully decomposed.</p>
<fig id="F2" position="float">
<label>FIGURE 2</label>
<caption>
<p>Morphology of Si<sub>3</sub>N<sub>4w</sub> after decarbonization: <bold>(A)</bold> macro photo; <bold>(B)</bold> SEM photo.</p>
</caption>
<graphic xlink:href="fmats-07-588716-g002.tif"/>
</fig>
<p>The Si<sub>3</sub>N<sub>4w</sub> volume fractions, bulk densities, and open porosities of the five prepared Si<sub>3</sub>N<sub>4w</sub> preforms after decarbonization are listed in <xref ref-type="table" rid="T1">Table 1</xref>. The Si<sub>3</sub>N<sub>4w</sub> volume fractions of the five preforms all increased due to the inevitable shrinkage during the solidification and decarbonization processes. Lower Si<sub>3</sub>N<sub>4w</sub> volume fractions in the sizing agent led to larger increasing rates of Si<sub>3</sub>N<sub>4w</sub> volume fractions in the preforms after decarbonization. In turn, the increase in the actual Si<sub>3</sub>N<sub>4w</sub> volume fraction in the preform led to a rise in bulk density from 0.42 to 1.50&#xa0;g/cm<sup>3</sup>. By comparison, the open porosity declined from 86.5 to 52.7&#xa0;vol%. The close porosity of the five preforms were all approximately 1&#xa0;vol%, confirming the high connectivity of pores inside the preforms.</p>
<table-wrap id="T1" position="float">
<label>TABLE 1</label>
<caption>
<p>Si<sub>3</sub>N<sub>4w</sub> volume fraction, bulk density, and open porosity of the five kinds of Si<sub>3</sub>N<sub>4w</sub> preform after decarbonization.</p>
</caption>
<table frame="hsides" rules="groups">
<thead>
<tr>
<th>Si<sub>3</sub>N<sub>4w</sub> volume fraction in size agent (vol%)</th>
<th align="center">Si<sub>3</sub>N<sub>4w</sub> volume fraction in preform after decarbonization (vol%)</th>
<th align="center">Bulk density (g/cm<sup>3</sup>)</th>
<th align="center">Open porosity (vol%)</th>
<th align="center">Close porosity (vol%)</th>
</tr>
</thead>
<tbody>
<tr>
<td>5</td>
<td align="center">13.0</td>
<td align="center">0.42</td>
<td align="center">86.5</td>
<td align="center">0.5</td>
</tr>
<tr>
<td>15</td>
<td align="center">19.9</td>
<td align="center">0.64</td>
<td align="center">79.7</td>
<td align="center">0.4</td>
</tr>
<tr>
<td>25</td>
<td align="center">29.2</td>
<td align="center">0.93</td>
<td align="center">69.5</td>
<td align="center">1.3</td>
</tr>
<tr>
<td>35</td>
<td align="center">38.5</td>
<td align="center">1.23</td>
<td align="center">60.3</td>
<td align="center">1.2</td>
</tr>
<tr>
<td>45</td>
<td align="center">46.8</td>
<td align="center">1.50</td>
<td align="center">52.7</td>
<td align="center">0.5</td>
</tr>
</tbody>
</table>
</table-wrap>
<p>The weight increasing rates of five Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> composites are presented in <xref ref-type="fig" rid="F3">Figure 3</xref>. All Si<sub>3</sub>N<sub>4</sub> matrices were almost incremented in the first furnace deposition. Thus, the diffusion channels of deposition gas in the preforms became closed after the process. The subsequent deposition process ensured complete densification of all five Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> under the deposition conditions. Lower Si<sub>3</sub>N<sub>4w</sub> volume fractions led to larger weight increasing rates of Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub>, as well as significant differences between different Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub>. The weight increasing rate of 5&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> in the first furnace deposition reached 200.85%, while that of 45&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> was only 5.09%. The reason for this had to do with the light weight and large porosity of the low Si<sub>3</sub>N<sub>4w</sub> volume fraction composite.</p>
<fig id="F3" position="float">
<label>FIGURE 3</label>
<caption>
<p>Weight increase rate of five kinds of Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub>.</p>
</caption>
<graphic xlink:href="fmats-07-588716-g003.tif"/>
</fig>
<p>The bulk densities and open porosities of five prepared Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> composites are depicted in <xref ref-type="fig" rid="F4">Figure 4</xref>. The bulk density of 5&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> was larger than that of 15&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub>. For other samples, larger Si<sub>3</sub>N<sub>4w</sub> volume fractions induced elevated bulk densities. The highest bulk density was recorded with 45&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> (1.65&#xa0;g/cm<sup>3</sup>), while the lowest was obtained with 15&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> (1.06&#xa0;g/cm<sup>3</sup>). The general rule of open porosity stated that higher Si<sub>3</sub>N<sub>4w</sub> volume fractions should yield larger open porosities. However, the high open porosity of 45&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> appeared to contradict the low porosity and small pore size of the 45&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub> preform.</p>
<fig id="F4" position="float">
<label>FIGURE 4</label>
<caption>
<p>Bulk density and open porosity of five kinds of Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub>.</p>
</caption>
<graphic xlink:href="fmats-07-588716-g004.tif"/>
</fig>
<p>To explain the above abnormal phenomenon, the surface morphologies of 45 and 25&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> were studied and the results are gathered in <xref ref-type="fig" rid="F5">Figure 5</xref>. Numerous cracks were distributed on the surface of 45&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> (<xref ref-type="fig" rid="F5">Figures 5B</xref>). The widths of the cracks were around 100&#xa0;nm (<xref ref-type="fig" rid="F5">Figures 5B</xref>). However, no cracks were noticed on the surface of 25&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> (<xref ref-type="fig" rid="F5">Figures 5C, D</xref>). Therefore, the surface cracks caused the elevated open porosity of 45&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub>. The difference between the crystalline Si<sub>3</sub>N<sub>4w</sub> and amorphous CVI Si<sub>3</sub>N<sub>4</sub> matrix (<xref ref-type="bibr" rid="B23">Zhou et al., 2019b</xref>) should induce differences between the thermal expansion coefficients of Si<sub>3</sub>N<sub>4w</sub> and the Si<sub>3</sub>N<sub>4</sub> matrix. Elevated Si<sub>3</sub>N<sub>4w</sub> volume fractions yielded larger differences. Thus, high Si<sub>3</sub>N<sub>4w</sub> volume fraction composites were more prone to surface cracking. The existence of surface cracking would inevitably cause stress concentration and high open porosity, which would decline the ability of rain erosion resistance. On the other hand, the thermal expansion coefficient mismatch brought by the change in the Si<sub>3</sub>N<sub>4w</sub> volume fraction should be taken into consideration during the preparation of wave-transparent composites.</p>
<fig id="F5" position="float">
<label>FIGURE 5</label>
<caption>
<p>Surface morphology of 45 and 25&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub>: <bold>(A)</bold> surface crack distribution of 45&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub>; <bold>(B)</bold> surface crack width of 45&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub>; <bold>(C)</bold> surface crack distribution of 25&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub>; <bold>(D)</bold> surface morphology of 25&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub>.</p>
</caption>
<graphic xlink:href="fmats-07-588716-g005.tif"/>
</fig>
<p>Assuming the density of both Si<sub>3</sub>N<sub>4w</sub> and the Si<sub>3</sub>N<sub>4</sub> matrix as 3.2&#xa0;g/cm<sup>3</sup>, the volume fraction of whisker, matrix, open pore, and close pore of the five prepared Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> composites through weight, bulk density, and open porosity were all obtained. In <xref ref-type="fig" rid="F6">Figure 6</xref>, the volume fractions of the solid phase of Si<sub>3</sub>N<sub>4w</sub> and the matrix were proportional to bulk densities in <xref ref-type="fig" rid="F4">Figure 4</xref>. Lower Si<sub>3</sub>N<sub>4w</sub> volume fractions led to elevated relative contents of the matrix. In turn, higher relative contents of the matrix represented superior load transfer capacities.</p>
<fig id="F6" position="float">
<label>FIGURE 6</label>
<caption>
<p>The volume fraction of open pores, closed pores, whisker, and matrix/vol%.</p>
</caption>
<graphic xlink:href="fmats-07-588716-g006.tif"/>
</fig>
<p>Typical macromorphologies of the Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> samples are displayed in <xref ref-type="fig" rid="F7">Figure 7</xref>. The surface of 25&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> looked evenly white with a hard texture (<xref ref-type="fig" rid="F7">Figures 7A</xref>). The thickness of 25&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> was estimated to be approximately 2&#xa0;mm (<xref ref-type="fig" rid="F7">Figures 7B</xref>). Also, two dividing centrosymmetric lines were noticed and both estimated to 0.5&#xa0;mm from the surface. This confirmed the limited penetration depth of the Si<sub>3</sub>N<sub>4</sub> matrix in a specific gel-casting Si<sub>3</sub>N<sub>4w</sub> preform under the CVI Si<sub>3</sub>N<sub>4</sub> process.</p>
<fig id="F7" position="float">
<label>FIGURE 7</label>
<caption>
<p>Typical macromorphology of Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub>: <bold>(A)</bold> surface of the 25&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub>; <bold>(B)</bold> section of the 25&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub>.</p>
</caption>
<graphic xlink:href="fmats-07-588716-g007.tif"/>
</fig>
<p>Based on the penetration morphology of <xref ref-type="fig" rid="F7">Figures 7B</xref>, the structure of Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> was simplified as a sandwich construction. The inherent characteristics of the CVI process caused a gradual decline in the content from the surface to the dividing line. The medium part was mainly composed of Si<sub>3</sub>N<sub>4w</sub> with almost no deposited matrix. This structure was similar to the A sandwich structure of a multi-layered radome structure consisting of a high-density side layer and low-density center layer. Materials with sandwich structures often possess high specific strengths and broadband wave-transparent abilities. Meanwhile, the gradient structure of the side layers relieved the stress, which may improve the mechanical properties of the materials. In other words, the whisker preform combined with the CVI process could yield materials with A sandwich and gradient structures.</p>
<p>The section penetration morphologies of the five prepared Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> ceramics are depicted in <xref ref-type="fig" rid="F8">Figure 8</xref>. Four positions (surface, 100, 500, and 1,000&#xa0;&#x3bc;m distance from the surface) were observed for each sample, and the yellow numbers represent the thickness of the matrix around Si<sub>3</sub>N<sub>4w</sub>. The surfaces of the five prepared Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> were all covered by dense CVI Si<sub>3</sub>N<sub>4</sub>. Each Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> sample revealed that closure of the surface led to less matrix content around Si<sub>3</sub>N<sub>4w</sub>. When the surface is closed, gas cannot enter the preform through the pores, resulting in a reduction of the internal matrix phase. At the same depth, larger Si<sub>3</sub>N<sub>4w</sub> volume fractions induced less matrix content around Si<sub>3</sub>N<sub>4w</sub>. For example, matrix deposition is rarely observed at 35 and 45&#xa0;vol%. With the increase of the whisker volume fraction, the amount of matrix decreases and the density changes. And the porosity increases gradually. More matrix was still deposited at 1&#xa0;mm distance from the surface in 5 and 15&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> samples. Likewise, the density and porosity decreased, but this is exactly what is needed to form the sandwich structure mentioned later. By comparison, almost no matrix surrounded Si<sub>3</sub>N<sub>4w</sub> at only 100&#xa0;&#x3bc;m distance from the surface in 15&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub>.</p>
<fig id="F8" position="float">
<label>FIGURE 8</label>
<caption>
<p>Section penetration morphology of five kinds of Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub>.</p>
</caption>
<graphic xlink:href="fmats-07-588716-g008.tif"/>
</fig>
<p>The pore size distributions of Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> are gathered in <xref ref-type="fig" rid="F9">Figure 9</xref>. The pore sizes of all five Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> specimens looked normally distributed. As Si<sub>3</sub>N<sub>4w</sub> volume fraction decreased, the pore size became more concentrated at 500, 600, 800, 1,600, and 2,500&#xa0;nm, respectively. Moreover, lower Si<sub>3</sub>N<sub>4w</sub> volume fractions induced wider pore size distribution ranges. Therefore, the A sandwich structure of Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> showed that the CVI Si<sub>3</sub>N<sub>4</sub> process could not effectively penetrate pores smaller than 2.5&#xa0;&#x3bc;m in a gel-casting Si<sub>3</sub>N<sub>4w</sub> preform.</p>
<fig id="F9" position="float">
<label>FIGURE 9</label>
<caption>
<p>Pore size distribution of Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub>.</p>
</caption>
<graphic xlink:href="fmats-07-588716-g009.tif"/>
</fig>
</sec>
<sec id="s3-2">
<title>Mechanical Properties</title>
<p>The flexural strengths of the five Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> composites were tested and the results are shown in <xref ref-type="fig" rid="F10">Figure 10</xref>. As the Si<sub>3</sub>N<sub>4w</sub> volume fraction increased, the flexural strength of Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> first rose and then decreased. A maximum strength of 41.37&#xa0;MPa was recorded with 25&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub>. The minimum flexural strength of 22.74&#xa0;MPa was registered with 45&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub>. The flexural strengths of different Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> composites were analyzed by combining the component volume fractions shown in <xref ref-type="fig" rid="F6">Figure 6</xref> and section penetration morphologies in <xref ref-type="fig" rid="F8">Figure 8</xref>. The 5 and 15&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> composites showed higher load transfer abilities due to elevated matrix contents. Therefore, apparent fractures of Si<sub>3</sub>N<sub>4w</sub> can still be seen at 1&#xa0;mm from the surface. However, the low Si<sub>3</sub>N<sub>4w</sub> volume fractions of 5 and 15&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> led to relatively lower flexural strengths. For 35 and 45&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub>, although they possessed elevated Si<sub>3</sub>N<sub>4w</sub> volume fractions, their low load transfer abilities caused by low matrix content significantly decreased their flexural strengths. Furthermore, the flexural strengths of 35 and 45&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> were a little lower than those of 5 and 15&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub>, confirming the significant influence of the load transfer ability of the matrix on flexural strength. By contrast, the 25&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> ceramic integrated a moderate whisker volume fraction and matrix content, thereby inducing a better strengthening effect and load transfer ability. When the volume fraction of the matrix is too low, the matrix cannot effectively bond and disperse the load, which leads to a decrease of strength. Similarly, when the volume fraction of the whisker is too low, the ability to hinder cracks and other defects is very small and cannot play an enhancement role, resulting in the reduction of strength. However, the volume fraction of 25&#xa0;vol% is in an intermediate state, which ensures the action of both the matrix and the reinforcer. This, in turn, led to the highest flexural strength.</p>
<fig id="F10" position="float">
<label>FIGURE 10</label>
<caption>
<p>Flexural strength of the five kinds of Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub>.</p>
</caption>
<graphic xlink:href="fmats-07-588716-g010.tif"/>
</fig>
<p>A typical fracture morphology of Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> is presented in <xref ref-type="fig" rid="F11">Figure 11</xref>. Numerous flat sections can be seen in the low magnification SEM photo. The high magnification photo showed a smooth interface between Si<sub>3</sub>N<sub>4w</sub> and the Si<sub>3</sub>N<sub>4</sub> matrix. Obviously, the fracture of Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> looked typically brittle, inferring the high bonding strength between Si<sub>3</sub>N<sub>4w</sub> and the Si<sub>3</sub>N<sub>4</sub> matrix.</p>
<fig id="F11" position="float">
<label>FIGURE 11</label>
<caption>
<p>Typical fracture morphology of Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub>: <bold>(A)</bold> low magnification SEM photo; <bold>(B)</bold> high magnification SEM photo.</p>
</caption>
<graphic xlink:href="fmats-07-588716-g011.tif"/>
</fig>
<p>The fracture toughness values of the five Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> samples were tested by a single-notched beam method and the data are gathered in <xref ref-type="fig" rid="F12">Figure 12</xref>. The high porosity and hollow sandwich structure of the composites led to very low fracture toughness values. As the Si<sub>3</sub>N<sub>4w</sub> volume fraction increased, the fracture toughness first fell and then rose. The highest value reached only 0.44&#xa0;MPa&#xa0;m<sup>1/2</sup> and was recorded with 45&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub>. By comparing the tendency with the component volume fraction in <xref ref-type="fig" rid="F6">Figure 6</xref>, the fracture toughness was shown to positively correlate with the total solid content of Si<sub>3</sub>N<sub>4w</sub> and the Si<sub>3</sub>N<sub>4</sub> matrix. From another perspective, the fracture toughness negatively correlated with porosity due to the very large bonding strength of the interface of Si<sub>3</sub>N<sub>4w</sub> and the Si<sub>3</sub>N<sub>4</sub> matrix, which prevented cracks from deflection. As a result, larger porosity led to lower fraction toughness.</p>
<fig id="F12" position="float">
<label>FIGURE 12</label>
<caption>
<p>Fracture toughness of the five kinds of Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub>.</p>
</caption>
<graphic xlink:href="fmats-07-588716-g012.tif"/>
</fig>
</sec>
<sec id="s3-3">
<title>Dielectric Properties</title>
<p>The room-temperature dielectric properties of the five Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> specimens are shown in <xref ref-type="fig" rid="F13">Figure 13</xref>. The dielectric constant ranged between 2.25 and 4.0, and was positively correlated with the total solid content in <xref ref-type="fig" rid="F8">Figure 8</xref>. Therefore, the relative content of the whisker and matrix did not influence the dielectric constant very much. As the whisker volume increases, the real part of the complex dielectric constant increases. From the perspective of the microstructure, with the whisker volume increasing, the pore radius decreases, and the electromagnetic wave scattering in the pore increases. So the dielectric constant increases as the dielectric loss also increases. Also, the dielectric constant values of the Si<sub>3</sub>N<sub>4</sub> matrix and Si<sub>3</sub>N<sub>4w</sub> were similar. The dielectric constant lines were approximately straight, showing a slight influence of frequency in the x-band on the dielectric constant.</p>
<fig id="F13" position="float">
<label>FIGURE 13</label>
<caption>
<p>Dielectric properties of the five kinds of Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub>.</p>
</caption>
<graphic xlink:href="fmats-07-588716-g013.tif"/>
</fig>
<p>Limited by the accuracy of the vector network analyzer during testing low-loss materials, the dielectric loss of the five Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> did not follow obvious rules. However, the dielectric loss of all five composites was less than 0.005, confirming excellent dielectric properties. Besides, the influences of the interface between the Si<sub>3</sub>N<sub>4</sub> matrix and Si<sub>3</sub>N<sub>4w</sub> on dielectric loss were slight.</p>
</sec>
</sec>
<sec sec-type="conclusion" id="s4">
<title>Conclusion</title>
<p>The effects of the Si<sub>3</sub>N<sub>4w</sub> volume fraction on the microstructures, mechanical properties, and dielectric characteristics of Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> were all studies in this paper and the following conclusions could be drawn:<list list-type="order">
<list-item>
<p>The connectivity of pores in the Si<sub>3</sub>N<sub>4w</sub> preform prepared by the gel-casting process was good due to the small pore size which yielded Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> with an A sandwich structure. The relative matrix content of 5&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> was higher than that of 15&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub>. Higher Si<sub>3</sub>N<sub>4w</sub> volume fractions led to lower relative contents of the Si<sub>3</sub>N<sub>4</sub> matrix and less matrix distribution at the same depth. In the sample of the volume fraction of 25&#xa0;vol%, the content of the matrix and whisker was moderate, and the porosity was the lowest, which made it form an ideal sandwich structure.</p>
</list-item>
<list-item>
<p>Since 25&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> integrated a relatively higher Si<sub>3</sub>N<sub>4w</sub> volume fraction and load transfer ability of the matrix, the resulting flexural strength reached the highest value of 41.37&#xa0;MPa. At a distance of 100&#xa0;&#x3bc;m from the surface, the matrix thickness around the whisker could still reach 140&#xa0;nm. The high open porosity led to the low fraction toughness of Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub>. The obvious brittle fracture showed a very high interface bonding strength. Therefore, the fracture toughness of Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> was positively related to the total solid content. The surface of the sample with a 45&#xa0;vol% whisker also reflected a high density, and the bulk density tended to be the highest. As a result, the fracture toughness of 45&#xa0;vol% Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> was the highest (0.44&#xa0;MPa&#xa0;m<sup>1/2</sup>).</p>
</list-item>
<list-item>
<p>The dielectric constants of Si<sub>3</sub>N<sub>4w</sub>/Si<sub>3</sub>N<sub>4</sub> ranged between 2.25 and 4.0, and was positively related to the total solid content. This may infer similar dielectric constants of Si<sub>3</sub>N<sub>4w</sub> and the Si<sub>3</sub>N<sub>4</sub> matrix. Dielectric losses were all less than 0.005, showing good dielectric properties of the composites. Besides, the dielectric loss of the interface between Si<sub>3</sub>N<sub>4w</sub> and the Si<sub>3</sub>N<sub>4</sub> matrix was slight.</p>
</list-item>
</list>
</p>
</sec>
<sec id="s5">
<title>Data Availability Statement</title>
<p>The original contributions presented in the study are included in the article/supplementary material, further inquiries can be directed to the corresponding author.</p>
</sec>
<sec id="s6">
<title>Author Contributions</title>
<p>CC, YL, and WY carried out the concepts, design, definition of intelectual content, literature search data acquisition, data analysis and manuscript preparation. FY, JW, and QZ provided assistance for data accuisition, data analysis and statistical analysis. CC carried out literature search data acquisition and manuscript editing. YL and WY performed manuscript review. All authors have read and approved the content of the manuscript.</p>
</sec>
<sec id="s7">
<title>Funding</title>
<p>This work was supported by the National Key Research and Development Program of China (No. 2018YFB1106600), the Chinese National Foundation for Natural Sciences under Contracts (No.51672217, No.51572224), and the Fundamental Research Funds for the Central Universities (No. 3102019ghxm014).</p>
</sec>
<sec sec-type="COI-statement" id="s8">
<title>Conflict of Interest</title>
<p>The authors declare that the research was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.</p>
</sec>
</body>
<back>
<ref-list>
<title>References</title>
<ref id="B1">
<citation citation-type="book">
<person-group person-group-type="author">
<name>
<surname>Arakawa</surname>
<given-names>T.</given-names>
</name>
<name>
<surname>Mori</surname>
<given-names>T.</given-names>
</name>
<name>
<surname>Matsumoto</surname>
<given-names>Y.</given-names>
</name>
</person-group> (<year>1991</year>). <source>Silicon nitride sintered body and process for preparation thereof</source>. <comment>US Patent No 5017530</comment>

</citation>
</ref>
<ref id="B2">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Ashok</surname>
<given-names>K.</given-names>
</name>
<name>
<surname>Sharma</surname>
<given-names>S.</given-names>
</name>
<name>
<surname>Ghanshyam</surname>
<given-names>S.</given-names>
</name>
</person-group> (<year>2007</year>). <article-title>Measurement of dielectric constant and loss factor of the dielectric material at microwave frequencies</article-title>. <source>Prog. Electromagn. Res. C</source> <volume>69</volume>, <fpage>47</fpage>&#x2013;<lpage>54</lpage>. <pub-id pub-id-type="doi">10.2528/PIER06111204</pub-id> 
</citation>
</ref>
<ref id="B3">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Bolivar</surname>
<given-names>P. H.</given-names>
</name>
<name>
<surname>Brucherseifer</surname>
<given-names>M.</given-names>
</name>
<name>
<surname>Rivas</surname>
<given-names>J. G.</given-names>
</name>
</person-group> (<year>2003</year>). <article-title>Measurement of the dielectric constant and loss tangent of high dielectric-constant materials at terahertz frequencies</article-title>. <source>IEEE Trans. Microw. Theory Tech.</source> <volume>51</volume> (<issue>4</issue>), <fpage>1062</fpage>&#x2013;<lpage>1066</lpage>. <pub-id pub-id-type="doi">10.1109/tmtt.2003.809693</pub-id>. 
</citation>
</ref>
<ref id="B4">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Cao</surname>
<given-names>F.</given-names>
</name>
<name>
<surname>Fang</surname>
<given-names>Z. Y.</given-names>
</name>
<name>
<surname>Zhang</surname>
<given-names>C. R.</given-names>
</name>
</person-group> (<year>2013</year>). <article-title>High-temperature properties and associated structure evolution of continuous SiNO fiber-reinforced BN composites for wave transparency</article-title>. <source>Mater. Design.</source> <volume>43</volume>, <fpage>258</fpage>&#x2013;<lpage>263</lpage>. <pub-id pub-id-type="doi">10.1016/j.matdes.2012.07.037</pub-id>. 
</citation>
</ref>
<ref id="B5">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Cheng</surname>
<given-names>Z. L.</given-names>
</name>
<name>
<surname>Ye</surname>
<given-names>F.</given-names>
</name>
<name>
<surname>Liu</surname>
<given-names>Y.</given-names>
</name>
<name>
<surname>Qiao</surname>
<given-names>T.</given-names>
</name>
<name>
<surname>Li</surname>
<given-names>J.</given-names>
</name>
<name>
<surname>Qin</surname>
<given-names>H.</given-names>
</name>
<etal/>
</person-group> (<year>2019</year>). <article-title>Mechanical and dielectric properties of porous and wave-transparent Si<sub>3</sub>N<sub>4</sub>-Si<sub>3</sub>N<sub>4</sub> composite ceramics fabricated by 3D printing combined with chemical vapor infiltration</article-title>. <source>J. Adv. Ceram.</source> <volume>8</volume> (<issue>3</issue>), <fpage>399</fpage>&#x2013;<lpage>407</lpage>. <pub-id pub-id-type="doi">10.1007/s40145-019-0322-8</pub-id>. 
</citation>
</ref>
<ref id="B6">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Ding</surname>
<given-names>S.</given-names>
</name>
<name>
<surname>Zeng</surname>
<given-names>Y.</given-names>
</name>
<name>
<surname>Jiang</surname>
<given-names>D.</given-names>
</name>
</person-group> (<year>2007</year>). <article-title>Oxidation bonding of porous silicon nitride ceramics with high strength and low dielectric constant</article-title>. <source>Mater. Lett.</source> <volume>61</volume> (<issue>11-12</issue>), <fpage>2277</fpage>&#x2013;<lpage>2280</lpage>. <pub-id pub-id-type="doi">10.1016/j.matlet.2006.08.067</pub-id>. 
</citation>
</ref>
<ref id="B7">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Hehdari</surname>
<given-names>M. S.</given-names>
</name>
<name>
<surname>Ghezavati</surname>
<given-names>J.</given-names>
</name>
<name>
<surname>Abbasgholipour</surname>
<given-names>M.</given-names>
</name>
<name>
<surname>Mohammadi Alasti</surname>
<given-names>B.</given-names>
</name>
</person-group> (<year>2017</year>). <article-title>Various types of ceramics used in radome: a review</article-title>. <source>Sci. Iran. B</source> <volume>24</volume> (<issue>3</issue>), <fpage>1136</fpage>&#x2013;<lpage>1147</lpage>. <pub-id pub-id-type="doi">10.24200/sci.2017.4095</pub-id> 
</citation>
</ref>
<ref id="B8">
<citation citation-type="book">
<person-group person-group-type="author">
<name>
<surname>Hsieh</surname>
<given-names>M. Y.</given-names>
</name>
<name>
<surname>Mizuhara</surname>
<given-names>H.</given-names>
</name>
</person-group> (<year>1987</year>). <source>Silicon nitride having low dielectric constant</source>. <comment>US Patent 4708943</comment>

</citation>
</ref>
<ref id="B9">
<citation citation-type="book">
<person-group person-group-type="author">
<name>
<surname>Hsieh</surname>
<given-names>M. Y.</given-names>
</name>
</person-group> (<year>1987</year>). <source>Low dielectric loss silicon nitride base material</source>. <comment>US Patent 4654315</comment>

</citation>
</ref>
<ref id="B10">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Kandi</surname>
<given-names>K. K.</given-names>
</name>
<name>
<surname>Thallapalli</surname>
<given-names>N.</given-names>
</name>
<name>
<surname>Chilakalapalli</surname>
<given-names>S. P. R.</given-names>
</name>
</person-group> (<year>2014</year>). <article-title>Devolopment of silicon nitride-based ceramic radomes-A review</article-title>. <source>Int. J. Appl. Ceram. Technol.</source> <volume>12</volume>, <fpage>909</fpage>&#x2013;<lpage>920</lpage>. <pub-id pub-id-type="doi">10.1111/ijac.12305</pub-id> 
</citation>
</ref>
<ref id="B11">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Lee</surname>
<given-names>S. W.</given-names>
</name>
<name>
<surname>Chae</surname>
<given-names>H. B.</given-names>
</name>
<name>
<surname>Park</surname>
<given-names>D. S.</given-names>
</name>
<name>
<surname>Choa</surname>
<given-names>Y. H.</given-names>
</name>
<name>
<surname>Niihara</surname>
<given-names>K.</given-names>
</name>
<name>
<surname>Hockey</surname>
<given-names>B. J.</given-names>
</name>
</person-group> (<year>2000</year>). <article-title>Thermal conductivity of unidirectionally oriented Si<sub>3</sub>N<sub>4</sub>w/Si<sub>3</sub>N<sub>4</sub> composites</article-title>. <source>J. Mater. Sci.</source> <volume>35</volume> (<issue>18</issue>), <fpage>4487</fpage>&#x2013;<lpage>4493</lpage>. <pub-id pub-id-type="doi">10.1023/A:1004807516791</pub-id> 
</citation>
</ref>
<ref id="B12">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Hou</surname>
<given-names>Y. B.</given-names>
</name>
<name>
<surname>Yang</surname>
<given-names>X. J.</given-names>
</name>
<name>
<surname>Li</surname>
<given-names>B.</given-names>
</name>
<name>
<surname>Lia</surname>
<given-names>D.</given-names>
</name>
<name>
<surname>Gaoa</surname>
<given-names>S.</given-names>
</name>
<name>
<surname>Wua</surname>
<given-names>Z.</given-names>
</name>
</person-group> (<year>2019</year>). <article-title>Preparation and interface modification of Si<sub>3</sub>N<sub>4f</sub>/SiO<sub>2</sub> composites</article-title>. <source>J. Mater. Sci. Technol.</source> <volume>35</volume> (<issue>12</issue>), <fpage>2767</fpage>&#x2013;<lpage>2771</lpage>. <pub-id pub-id-type="doi">10.1016/j.jmst.2019.05.069</pub-id>. 
</citation>
</ref>
<ref id="B13">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Li</surname>
<given-names>Z. Z.</given-names>
</name>
<name>
<surname>Zou</surname>
<given-names>Z. Y.</given-names>
</name>
<name>
<surname>Qin</surname>
<given-names>Y.</given-names>
</name>
<name>
<surname>Qi</surname>
<given-names>M.</given-names>
</name>
<name>
<surname>Ren</surname>
<given-names>J.</given-names>
</name>
<name>
<surname>Peng</surname>
<given-names>Z.</given-names>
</name>
</person-group> (<year>2020</year>). <article-title>The effect of fibre content on properties of ceramifiable composites</article-title>. <source>Plast. Rubber Compos.</source> <volume>49</volume>, <fpage>230</fpage>&#x2013;<lpage>236</lpage>. <pub-id pub-id-type="doi">10.1080/14658011.2020.1731258</pub-id> 
</citation>
</ref>
<ref id="B14">
<citation citation-type="book">
<person-group person-group-type="author">
<name>
<surname>Medding</surname>
<given-names>J. A.</given-names>
</name>
</person-group> (<year>1996</year>). <article-title>Nondestructive evaluation of zirconium phosphate bonded silicon nitride radomes</article-title>. <comment>Master&#x2019;s thesis</comment>. <publisher-loc>Blacksburg (VA)</publisher-loc>: <publisher-name>Virginia Polytechnic Institute and State University</publisher-name> 
</citation>
</ref>
<ref id="B15">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Qi</surname>
<given-names>G.</given-names>
</name>
<name>
<surname>Zhang</surname>
<given-names>C.</given-names>
</name>
<name>
<surname>Hu</surname>
<given-names>H.</given-names>
</name>
<name>
<surname>Cao</surname>
<given-names>F.</given-names>
</name>
<name>
<surname>Wang</surname>
<given-names>S.</given-names>
</name>
<name>
<surname>Jiang</surname>
<given-names>Y.</given-names>
</name>
</person-group> (<year>2005a</year>). <article-title>Crystallization behavior of three-dimensional silica fiber reinforced silicon nitride composite</article-title>. <source>J. Cryst. Growth.</source> <volume>284</volume> (<issue>1-2</issue>), <fpage>293</fpage>&#x2013;<lpage>296</lpage>. <pub-id pub-id-type="doi">10.1016/j.jcrysgro.2005.06.039</pub-id>. 
</citation>
</ref>
<ref id="B16">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Qi</surname>
<given-names>G. J.</given-names>
</name>
<name>
<surname>Zhang</surname>
<given-names>C. R.</given-names>
</name>
<name>
<surname>Hu</surname>
<given-names>H. F.</given-names>
</name>
<name>
<surname>Cao</surname>
<given-names>S. F.</given-names>
</name>
<name>
<surname>Wang</surname>
<given-names>Q.</given-names>
</name>
<name>
<surname>Cao</surname>
<given-names>Y. B.</given-names>
</name>
</person-group> (<year>2005b</year>). <article-title>Preparation of three-dimensional silica fiber reinforced silicon nitride composites using perhydropolysilazane as precursor</article-title>. <source>Mater. Lett.</source> <volume>59</volume> (<issue>26</issue>), <fpage>3256</fpage>&#x2013;<lpage>3258</lpage>. <pub-id pub-id-type="doi">10.1016/j.matlet.2005.04.057</pub-id>. 
</citation>
</ref>
<ref id="B17">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Qi</surname>
<given-names>G.</given-names>
</name>
<name>
<surname>Zhang</surname>
<given-names>C.</given-names>
</name>
<name>
<surname>Hu</surname>
<given-names>H.</given-names>
</name>
<name>
<surname>Cao</surname>
<given-names>F.</given-names>
</name>
<name>
<surname>Wang</surname>
<given-names>S. S.</given-names>
</name>
<name>
<surname>Jiang</surname>
<given-names>Y.</given-names>
</name>
</person-group> (<year>2005c</year>). <article-title>Three-dimensional silica fiber reinforced silicon nitride&#x2010;based composites fabricated via different polysilazanes</article-title>. <source>Adv. Eng. Mater.</source> <volume>7</volume> (<issue>11</issue>), <fpage>1043</fpage>&#x2013;<lpage>1046</lpage>. <pub-id pub-id-type="doi">10.1002/adem.200500104</pub-id>. 
</citation>
</ref>
<ref id="B18">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Wan</surname>
<given-names>W.</given-names>
</name>
<name>
<surname>Feng</surname>
<given-names>Y. B.</given-names>
</name>
<name>
<surname>Yang</surname>
<given-names>J.</given-names>
</name>
<name>
<surname>Bu</surname>
<given-names>W.</given-names>
</name>
<name>
<surname>Qiu</surname>
<given-names>T.</given-names>
</name>
</person-group> (<year>2016</year>). <article-title>Microstructure, mechanical and high-temperature dielectric properties of zirconia-reinforced fused silica ceramics</article-title>. <source>Ceram. Int.</source> <volume>42</volume> (<issue>5</issue>), <fpage>6436</fpage>&#x2013;<lpage>6443</lpage>. <pub-id pub-id-type="doi">10.1016/j.ceramint.2016.01.063</pub-id>. 
</citation>
</ref>
<ref id="B19">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Xu</surname>
<given-names>H. H. K.</given-names>
</name>
<name>
<surname>Ostertag</surname>
<given-names>C. P.</given-names>
</name>
<name>
<surname>Braun</surname>
<given-names>L. M.</given-names>
</name>
<name>
<surname>Lloyd</surname>
<given-names>I. K.</given-names>
</name>
</person-group> (<year>1994</year>). <article-title>Effects of fiber volume fraction on mechanical properties of SiC-fiber/Si<sub>3</sub>N<sub>4</sub>-matrix composites</article-title>. <source>J. Am. Ceram. Soc.</source> <volume>77</volume> (<issue>7</issue>), <fpage>1897</fpage>&#x2013;<lpage>1900</lpage>. <pub-id pub-id-type="doi">10.1111/j.1151-2916.1994.tb07068.x</pub-id>. 
</citation>
</ref>
<ref id="B20">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Xu</surname>
<given-names>J.</given-names>
</name>
<name>
<surname>Luo</surname>
<given-names>F.</given-names>
</name>
<name>
<surname>Zhou</surname>
<given-names>W. C.</given-names>
</name>
</person-group> (<year>2020</year>). <article-title>Dielectric properties of porous reaction-bonded silicon nitride with different additives[J]</article-title>. <source>J. Electron. Mater.</source> <volume>49</volume> (<issue>3</issue>), <fpage>1611</fpage>&#x2013;<lpage>1617</lpage>. <pub-id pub-id-type="doi">10.1007/s11664-019-07462-6</pub-id>. 
</citation>
</ref>
<ref id="B21">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Yang</surname>
<given-names>X. J.</given-names>
</name>
<name>
<surname>Li</surname>
<given-names>B.</given-names>
</name>
<name>
<surname>Li</surname>
<given-names>D.</given-names>
</name>
<name>
<surname>Shao</surname>
<given-names>C.</given-names>
</name>
<name>
<surname>Zhang</surname>
<given-names>C.</given-names>
</name>
</person-group> (<year>2019</year>). <article-title>High-temperature properties and interface evolution of silicon nitride fiber reinforced silica matrix wave-transparent composite materials</article-title>. <source>J. Eur. Ceram. Soc.</source> <volume>39</volume>, <fpage>240</fpage>&#x2013;<lpage>248</lpage>. <pub-id pub-id-type="doi">10.1016/j.jeurceramsoc.2018.09.007</pub-id>. 
</citation>
</ref>
<ref id="B22">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Zhou</surname>
<given-names>J.</given-names>
</name>
<name>
<surname>Cheng</surname>
<given-names>L.</given-names>
</name>
<name>
<surname>Ye</surname>
<given-names>F.</given-names>
</name>
<name>
<surname>Zhang</surname>
<given-names>L.</given-names>
</name>
<name>
<surname>Liu</surname>
<given-names>Y.</given-names>
</name>
<name>
<surname>Cui</surname>
<given-names>X.</given-names>
</name>
<etal/>
</person-group> (<year>2019a</year>). <article-title>Effects of heat treatment on mechanical and dielectric properties of 3D Si3N4f/BN/Si3N4 composite by CVI</article-title>. <source>J. Eur. Ceram. Soc.</source> <volume>40</volume> (<issue>15</issue>), <fpage>5305</fpage>&#x2013;<lpage>5315</lpage>. <pub-id pub-id-type="doi">10.1016/j.jeurceramsoc.2020.06.018</pub-id> 
</citation>
</ref>
<ref id="B23">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Zhou</surname>
<given-names>J.</given-names>
</name>
<name>
<surname>Ye</surname>
<given-names>F.</given-names>
</name>
<name>
<surname>Cheng</surname>
<given-names>L.</given-names>
</name>
<name>
<surname>li</surname>
<given-names>M.</given-names>
</name>
<name>
<surname>Yue</surname>
<given-names>W.</given-names>
</name>
<name>
<surname>Wang</surname>
<given-names>Y.</given-names>
</name>
</person-group> (<year>2019b</year>). <article-title>Microstructure and mechanical properties of Si3N4f/Si3N4 composites with different coatings</article-title>. <source>Ceram. Int.</source> <volume>45</volume> (<issue>10</issue>), <fpage>13308</fpage>&#x2013;<lpage>13314</lpage>. <pub-id pub-id-type="doi">10.1016/j.ceramint.2019.04.020</pub-id>. 
</citation>
</ref>
<ref id="B24">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Zou</surname>
<given-names>B.</given-names>
</name>
<name>
<surname>Huang</surname>
<given-names>C.</given-names>
</name>
<name>
<surname>Chena</surname>
<given-names>M.</given-names>
</name>
</person-group> (<year>2009</year>). <article-title>Study on the mechanical properties, microstructure and oxidation resistance of Si3N4/Si3N4W/Ti(C7N3) nanocomposites ceramic tool materials</article-title>. <source>Int. J. Refract. Metals Hard Mater.</source> <volume>27</volume> (<issue>1</issue>), <fpage>52</fpage>&#x2013;<lpage>60</lpage>. <pub-id pub-id-type="doi">10.1016/j.ijrmhm.2008.03.003</pub-id>. 
</citation>
</ref>
</ref-list>
</back>
</article>