<?xml version="1.0" encoding="UTF-8"?>
<!DOCTYPE article PUBLIC "-//NLM//DTD Journal Publishing DTD v2.3 20070202//EN" "journalpublishing.dtd">
<article article-type="research-article" dtd-version="2.3" xml:lang="EN" xmlns:mml="http://www.w3.org/1998/Math/MathML" xmlns:xlink="http://www.w3.org/1999/xlink">
<front>
<journal-meta>
<journal-id journal-id-type="publisher-id">Front. Mater.</journal-id>
<journal-title>Frontiers in Materials</journal-title>
<abbrev-journal-title abbrev-type="pubmed">Front. Mater.</abbrev-journal-title>
<issn pub-type="epub">2296-8016</issn>
<publisher>
<publisher-name>Frontiers Media S.A.</publisher-name>
</publisher>
</journal-meta>
<article-meta>
<article-id pub-id-type="publisher-id">934215</article-id>
<article-id pub-id-type="doi">10.3389/fmats.2022.934215</article-id>
<article-categories>
<subj-group subj-group-type="heading">
<subject>Materials</subject>
<subj-group>
<subject>Original Research</subject>
</subj-group>
</subj-group>
</article-categories>
<title-group>
<article-title>High Temperature Oxidation Behavior of Nano-Alumina&#x2013;Modified NiAl Coating</article-title>
<alt-title alt-title-type="left-running-head">Fang et al.</alt-title>
<alt-title alt-title-type="right-running-head">Alumina-Modified NiAl Coating</alt-title>
</title-group>
<contrib-group>
<contrib contrib-type="author">
<name>
<surname>Fang</surname>
<given-names>Yuqing</given-names>
</name>
<xref ref-type="aff" rid="aff1">
<sup>1</sup>
</xref>
<xref ref-type="aff" rid="aff2">
<sup>2</sup>
</xref>
<uri xlink:href="https://loop.frontiersin.org/people/1807331/overview"/>
</contrib>
<contrib contrib-type="author" corresp="yes">
<name>
<surname>Shu</surname>
<given-names>Xiaoyong</given-names>
</name>
<xref ref-type="aff" rid="aff1">
<sup>1</sup>
</xref>
<xref ref-type="aff" rid="aff2">
<sup>2</sup>
</xref>
<xref ref-type="corresp" rid="c001">&#x2a;</xref>
<uri xlink:href="https://loop.frontiersin.org/people/1795189/overview"/>
</contrib>
<contrib contrib-type="author">
<name>
<surname>Dong</surname>
<given-names>Shuhe</given-names>
</name>
<xref ref-type="aff" rid="aff1">
<sup>1</sup>
</xref>
<xref ref-type="aff" rid="aff2">
<sup>2</sup>
</xref>
</contrib>
</contrib-group>
<aff id="aff1">
<sup>1</sup>
<institution>School of Materials Science and Engineering</institution>, <institution>Nanchang Hangkong University</institution>, <addr-line>Nanchang</addr-line>, <country>China</country>
</aff>
<aff id="aff2">
<sup>2</sup>
<institution>Jiangxi Aviation Material Surface Technology Engineering Center</institution>, <addr-line>Nanchang</addr-line>, <country>China</country>
</aff>
<author-notes>
<fn fn-type="edited-by">
<p>
<bold>Edited by:</bold> <ext-link ext-link-type="uri" xlink:href="https://loop.frontiersin.org/people/1520994/overview">Yi Xu</ext-link>, Nanchang University, China</p>
</fn>
<fn fn-type="edited-by">
<p>
<bold>Reviewed by:</bold> <ext-link ext-link-type="uri" xlink:href="https://loop.frontiersin.org/people/1804578/overview">Zenghua Gao</ext-link>, Aerospace Special Materials and Processing Technology Institute Beijing, China</p>
<p>
<ext-link ext-link-type="uri" xlink:href="https://loop.frontiersin.org/people/1807611/overview">Bo Li</ext-link>, East China University of Science and Technology, China</p>
</fn>
<corresp id="c001">&#x2a;Correspondence: Xiaoyong Shu, <email>xiaoyong202@126.com</email>
</corresp>
<fn fn-type="other">
<p>This article was submitted to Environmental Degradation of Materials, a section of the journal Frontiers in Materials</p>
</fn>
</author-notes>
<pub-date pub-type="epub">
<day>27</day>
<month>06</month>
<year>2022</year>
</pub-date>
<pub-date pub-type="collection">
<year>2022</year>
</pub-date>
<volume>9</volume>
<elocation-id>934215</elocation-id>
<history>
<date date-type="received">
<day>02</day>
<month>05</month>
<year>2022</year>
</date>
<date date-type="accepted">
<day>16</day>
<month>05</month>
<year>2022</year>
</date>
</history>
<permissions>
<copyright-statement>Copyright &#xa9; 2022 Fang, Shu and Dong.</copyright-statement>
<copyright-year>2022</copyright-year>
<copyright-holder>Fang, Shu and Dong</copyright-holder>
<license xlink:href="http://creativecommons.org/licenses/by/4.0/">
<p>This is an open-access article distributed under the terms of the Creative Commons Attribution License (CC BY). The use, distribution or reproduction in other forums is permitted, provided the original author(s) and the copyright owner(s) are credited and that the original publication in this journal is cited, in accordance with accepted academic practice. No use, distribution or reproduction is permitted which does not comply with these terms.</p>
</license>
</permissions>
<abstract>
<p>In this article, the nickel aluminide coating prepared by the chemical vapor deposition method has adhered deliberately with nano-alumina film on the surface by the electrophoresis method. The analysis results of oxidation behavior in the air at 1,000&#xb0;C reported that the nano-alumina particles adhering to the nickel aluminide coating surface appear to be effective in facilitating the &#x3b8;-Al<sub>2</sub>O<sub>3</sub> to &#x3b1;-Al<sub>2</sub>O<sub>3</sub> phase transformation. The fast &#x3b8; to &#x3b1; phase transformation helps reduce the oxidation rate of the nickel&#x2013;aluminum coating and prevents the cracking and peeling in the oxide scale. The research addressed a novel method to improve the high-temperature oxidation resistance of nickel aluminide coatings.</p>
</abstract>
<kwd-group>
<kwd>Nickel aluminide coating</kwd>
<kwd>alumina modified</kwd>
<kwd>high temperature</kwd>
<kwd>oxidation</kwd>
<kwd>phase transition</kwd>
</kwd-group>
</article-meta>
</front>
<body>
<sec id="s1">
<title>Introduction</title>
<p>Nickel aluminide coatings, such as NiAl and Ni<sub>2</sub>Al<sub>3</sub>, are generally applied to the surfaces of engine turbine components to lengthen their service life (<xref ref-type="bibr" rid="B6">Goward, 1970</xref>; <xref ref-type="bibr" rid="B5">Goward and Boone, 1971</xref>; <xref ref-type="bibr" rid="B9">Leng et al., 2020</xref>). The common preparation methods of nickel aluminide coatings include slurry, powder embedding, physical vapor deposition, and chemical vapor deposition (CVD) (<xref ref-type="bibr" rid="B13">Nicholls, 2003</xref>; <xref ref-type="bibr" rid="B3">Bouchaud et al., 2013</xref>; <xref ref-type="bibr" rid="B11">Mollard et al., 2013</xref>; <xref ref-type="bibr" rid="B12">Montero et al., 2013</xref>). Compared with the other methods, the coating prepared by the CVD method has a stronger bonding force with the substrate and is denser, so its high-temperature oxidation resistance is better (<xref ref-type="bibr" rid="B21">Warnes and Punola, 1997</xref>; <xref ref-type="bibr" rid="B23">Yavorska et al., 2011</xref>; <xref ref-type="bibr" rid="B4">Goral et al., 2020</xref>).</p>
<p>The surface of the nickel aluminide coating will form protective thermally grown oxide (TGO)-Al<sub>2</sub>O<sub>3</sub> at high temperatures (<xref ref-type="bibr" rid="B16">Swadba et al., 2011</xref>). Several types of Al<sub>2</sub>O<sub>3</sub> have been found on alloys forming aluminides, such as &#x3b3;-Al<sub>2</sub>O<sub>3</sub>, &#x3b4;-Al<sub>2</sub>O<sub>3</sub>, &#x3b8;-Al<sub>2</sub>O<sub>3</sub>, and &#x3b1;-Al<sub>2</sub>O<sub>3</sub>. &#x3b1;-Al<sub>2</sub>O<sub>3</sub> is a good protective oxide scale because of its thermodynamic stability and slow growth rate (<xref ref-type="bibr" rid="B2">An et al., 2000</xref>). During the oxidation at a temperature above 1,100&#xb0;C, the nickel aluminide coating quickly forms the thermodynamically stable &#x3b1;-Al<sub>2</sub>O<sub>3</sub> scale, while the metastable alumina variants scales (normally &#x3b3; and &#x3b8;) are formed after a oxidation for a long time (<xref ref-type="bibr" rid="B1">Khana et al., 2019</xref>) at a temperature below 1,100&#xb0;C, during which they always experience the phase transformation of metastable-to-stable alumina (<xref ref-type="bibr" rid="B14">Peng et al., 2003</xref>; <xref ref-type="bibr" rid="B8">Huang and Peng, 2016</xref>), such as &#x3b8;-to-&#x3b1;. This phase transformation accompanies a volume shrinkage of about 10%, sometimes resulting in the generation of micro-cracks in the alumina scale (<xref ref-type="bibr" rid="B14">Peng et al., 2003</xref>; <xref ref-type="bibr" rid="B18">Veal et al., 2006</xref>; <xref ref-type="bibr" rid="B20">Wang and Zhou, 2012</xref>; <xref ref-type="bibr" rid="B8">Huang and Peng, 2016</xref>).</p>
<p>As a result, prompting the conversion of metastable-to-stable alumina is advantageous for improving the oxidation resistance of nickel aluminide coatings at high temperatures (<xref ref-type="bibr" rid="B1">Khana et al., 2019</xref>). Moreover there is a well-known fact that a rising temperature causes a faster phase transformation of the metastable-to-stable alumina, dopants or template effects have been found to change this process (<xref ref-type="bibr" rid="B17">Tolpygo and Clarke, 2000</xref>; <xref ref-type="bibr" rid="B7">Huang et al., 2019</xref>). For instance, Pint and his co-workers (<xref ref-type="bibr" rid="B15">Pint et al., 1997</xref>; <xref ref-type="bibr" rid="B7">Huang et al., 2019</xref>) found that Y<sub>2</sub>O<sub>3</sub>, La<sub>2</sub>O<sub>3</sub>, ZrO<sub>2</sub>, and HfO<sub>2</sub> dispersions in &#x3b2;-NiAl tend to retard the &#x3b8;-to-&#x3b1; phase transformation, whereas TiO<sub>2</sub> dispersion appears to promote this process. Lately, Peng and his co-workers (<xref ref-type="bibr" rid="B22">Xu et al., 2010</xref>; <xref ref-type="bibr" rid="B8">Huang and Peng, 2016</xref>; <xref ref-type="bibr" rid="B19">Wang et al., 2016</xref>; <xref ref-type="bibr" rid="B1">Khana et al., 2019</xref>) reported the promoted formation of an &#x3b1;-Al<sub>2</sub>O<sub>3</sub> scale on nickel aluminide with surface Cr<sub>2</sub>O<sub>3</sub> particles. On these bases, we have a concept that spreading oxide particles (e.g., Cr<sub>2</sub>O<sub>3</sub>) with the same crystallographic structure as &#x3b1;-Al<sub>2</sub>O<sub>3</sub> to aluminide can promote the growth of an &#x3b1;-Al<sub>2</sub>O<sub>3</sub> scale at a high temperature (<xref ref-type="bibr" rid="B24">Yin and Zhen, 2015</xref>). Valet et al. (<xref ref-type="bibr" rid="B10">Liu et al., 2007</xref>; <xref ref-type="bibr" rid="B8">Huang and Peng, 2016</xref>; <xref ref-type="bibr" rid="B1">Khana et al., 2019</xref>) found that the remaining fine &#x3b1;-Al<sub>2</sub>O<sub>3</sub> grits, used for the polishing surface of the intermetallic sample, appeared to promote the nucleation of &#x3b1;-Al<sub>2</sub>O<sub>3</sub>.</p>
<p>In this article, nano-alumina particles were deposited on the surface of aluminide coatings by electrophoresis, and their effects on the phase transition and oxidation kinetics of the nickel aluminide coatings were investigated. It is aimed to better understand the phase transitions of the oxidative properties of nickel aluminides, and find a more effective way to improve the oxidation resistance of these nickel aluminide oxides by promoting the growth of &#x3b1;-Al<sub>2</sub>O<sub>3</sub>.</p>
</sec>
<sec id="s2">
<title>The Experiment</title>
<p>The pure nickel samples with dimensions of 10&#xa0;mm &#xd7; 10&#xa0;mm &#xd7; 2&#xa0;mm were cut from an electrolyte pure nickel plate. After being abraded to a final 2,000 grit SiC paper, they were ultrasonically cleaned in acetone. By using the CVD method, the Ni<sub>2</sub>Al<sub>3</sub> coating was developed on the pure nickel surface after aluminizing at 750&#xb0;C &#xd7; 200 torr for 3&#xa0;h. The preparation process is as follows: high-purity Cl<sub>2</sub> was injected into the reaction chamber containing high-purity aluminum particles (purity: 99.99%, size: 3&#xa0;mm) to generate gas-phase halide AlCl<sub>x</sub>. AlCl<sub>x</sub> was carried into the deposition chamber by Ar, and then was reduced to activity [Al] by H<sub>2</sub>. The [Al] deposited on the pure nickel, and reacted with nickel to form a nickel aluminum coating. After aluminizing for 3&#xa0;h, the samples were cooled to room temperature with the furnace. The main equations involved in the reaction are as follows:<disp-formula id="e1">
<mml:math id="m1">
<mml:mrow>
<mml:mn>2</mml:mn>
<mml:mtext>Al</mml:mtext>
<mml:mo>&#x2b;</mml:mo>
<mml:msub>
<mml:mtext>Cl2</mml:mtext>
<mml:mrow>
<mml:mo>(</mml:mo>
<mml:mtext>g</mml:mtext>
<mml:mo>)</mml:mo>
</mml:mrow>
</mml:msub>
<mml:mo>&#x2192;</mml:mo>
<mml:mn>2</mml:mn>
<mml:msub>
<mml:mtext>AlCl</mml:mtext>
<mml:mrow>
<mml:mo>(</mml:mo>
<mml:mtext>g</mml:mtext>
<mml:mo>)</mml:mo>
</mml:mrow>
</mml:msub>
<mml:mtext>,</mml:mtext>
</mml:mrow>
</mml:math>
<label>(1)</label>
</disp-formula>
<disp-formula id="e2">
<mml:math id="m2">
<mml:mrow>
<mml:mtext>Al</mml:mtext>
<mml:mo>&#x2b;</mml:mo>
<mml:msub>
<mml:mtext>Cl2</mml:mtext>
<mml:mrow>
<mml:mo>(</mml:mo>
<mml:mtext>g</mml:mtext>
<mml:mo>)</mml:mo>
</mml:mrow>
</mml:msub>
<mml:mo>&#x2192;</mml:mo>
<mml:msub>
<mml:mtext>AlCl2</mml:mtext>
<mml:mrow>
<mml:mo>(</mml:mo>
<mml:mtext>g</mml:mtext>
<mml:mo>)</mml:mo>
</mml:mrow>
</mml:msub>
<mml:mtext>,</mml:mtext>
</mml:mrow>
</mml:math>
<label>(2)</label>
</disp-formula>
<disp-formula id="e3">
<mml:math id="m3">
<mml:mrow>
<mml:mn>2</mml:mn>
<mml:mtext>Al</mml:mtext>
<mml:mo>&#x2b;</mml:mo>
<mml:msub>
<mml:mtext>3Cl2</mml:mtext>
<mml:mrow>
<mml:mo>(</mml:mo>
<mml:mtext>g</mml:mtext>
<mml:mo>)</mml:mo>
</mml:mrow>
</mml:msub>
<mml:mo>&#x2192;</mml:mo>
<mml:mn>2</mml:mn>
<mml:mtext>AlCl</mml:mtext>
<mml:msub>
<mml:mn>3</mml:mn>
<mml:mrow>
<mml:mo>(</mml:mo>
<mml:mtext>g</mml:mtext>
<mml:mo>)</mml:mo>
</mml:mrow>
</mml:msub>
<mml:mtext>,</mml:mtext>
</mml:mrow>
</mml:math>
<label>(3)</label>
</disp-formula>
<disp-formula id="e4">
<mml:math id="m4">
<mml:mrow>
<mml:msub>
<mml:mtext>AlCl&#xa0;</mml:mtext>
<mml:mrow>
<mml:mo>(</mml:mo>
<mml:mtext>g</mml:mtext>
<mml:mo>)</mml:mo>
</mml:mrow>
</mml:msub>
<mml:mo>&#x2b;</mml:mo>
<mml:msub>
<mml:mtext>&#xa0;AlCl2</mml:mtext>
<mml:mrow>
<mml:mo>(</mml:mo>
<mml:mtext>g</mml:mtext>
<mml:mo>)</mml:mo>
</mml:mrow>
</mml:msub>
<mml:mo>&#x2b;</mml:mo>
<mml:msub>
<mml:mtext>&#xa0;AlCl3</mml:mtext>
<mml:mrow>
<mml:mo>(</mml:mo>
<mml:mtext>g</mml:mtext>
<mml:mo>)</mml:mo>
</mml:mrow>
</mml:msub>
<mml:mo>&#x2b;</mml:mo>
<mml:msub>
<mml:mtext>3H2</mml:mtext>
<mml:mrow>
<mml:mo>(</mml:mo>
<mml:mtext>g</mml:mtext>
<mml:mo>)</mml:mo>
</mml:mrow>
</mml:msub>
<mml:mo>&#x2192;</mml:mo>
<mml:mn>3</mml:mn>
<mml:mrow>
<mml:mo>[</mml:mo>
<mml:mtext>Al</mml:mtext>
<mml:mo>]</mml:mo>
</mml:mrow>
<mml:mo>&#x2b;</mml:mo>
<mml:msub>
<mml:mtext>6HCl</mml:mtext>
<mml:mrow>
<mml:mo>(</mml:mo>
<mml:mtext>g</mml:mtext>
<mml:mo>)</mml:mo>
</mml:mrow>
</mml:msub>
<mml:mtext>.</mml:mtext>
</mml:mrow>
</mml:math>
<label>(4)</label>
</disp-formula>
</p>
<p>The nano-Al<sub>2</sub>O<sub>3</sub> film was made to adhere to the nickel aluminum coating surface by electrophoresis technology. High temperature oxidation experiments were performed using the SETSYS evolution thermo-gravimetric analyzer (for <italic>in situ</italic> recording oxidation curves) in the air at 1,000&#xb0;C for 50&#xa0;h. A nickel layer was coated on the oxide scale surface using electroplating in the acidic electroless nickel plating mixed solution (containing 25&#xa0;g/L C<sub>3</sub>H<sub>6</sub>O<sub>3</sub>, 6.25&#xa0;g/L Na<sub>2</sub>CO<sub>3</sub>, 43&#xa0;g/L NiSO<sub>4</sub>&#xb7;6H<sub>2</sub>O, and 25&#xa0;g/L NaH<sub>2</sub>PO<sub>2</sub>&#xb7;H<sub>2</sub>O) at 98&#xb0;C for 5&#xa0;h. Scanning electron microscope (SEM), energy dispersive spectroscopy (EDS), and X-ray diffraction (XRD) were used to investigate the surface and cross-section morphologies, structure, and the phases of various nickel aluminide coatings.</p>
</sec>
<sec sec-type="results|discussion" id="s3">
<title>Results and Discussion</title>
<p>The cross-sectional morphology (<xref ref-type="fig" rid="F1">Figure 1A</xref>) shows that a single layer of nickel aluminide coating (&#x223c;30&#xa0;&#xb5;m thickness) was deposited on pure nickel after aluminizing. The coating was dense and well adherent to the pure Ni substrate. The Ni content and Al content of the coating were 39.3 at.% and 58.9 at.%, respectively. The XRD result (<xref ref-type="fig" rid="F1">Figure 1C</xref>) characterized them as deposited coating as a &#x3b4;-Ni<sub>2</sub>Al<sub>3</sub> phase. Backscattered SEM images of the polished cross-section of a nano-Al<sub>2</sub>O<sub>3</sub> film sample are shown in <xref ref-type="fig" rid="F1">Figure 1B</xref>. The as-electrophoresis Al<sub>2</sub>O<sub>3</sub> film was continuous with a thickness of around 3&#xa0;&#xb5;m. However, the Al<sub>2</sub>O<sub>3</sub> film was partially detached from the coating due to grinding and polishing during the preparation process.</p>
<fig id="F1" position="float">
<label>FIGURE 1</label>
<caption>
<p>Cross-sectional morphologies of Ni<sub>2</sub>Al<sub>3</sub> coatings <bold>(A)</bold> naked, <bold>(B)</bold> with an Al<sub>2</sub>O<sub>3</sub> film on the surface, and <bold>(C)</bold> XRD pattern of the naked Ni<sub>2</sub>Al<sub>3</sub> coating.</p>
</caption>
<graphic xlink:href="fmats-09-934215-g001.tif"/>
</fig>
<p>
<xref ref-type="fig" rid="F2">Figure 2</xref> shows the dependence on the time of mass grain and the square of mass grain of naked and Al<sub>2</sub>O<sub>3</sub> film-covered Ni<sub>2</sub>Al<sub>3</sub> coatings oxidated at 1,000&#xb0;C for 50&#xa0;h. The mass grain of Al<sub>2</sub>O<sub>3</sub> film-covered Ni<sub>2</sub>Al<sub>3</sub> coating is less than that of the naked one as shown in <xref ref-type="fig" rid="F2">Figure 2A</xref>. In the early stages of oxidation , the surface of the two types of coatings quickly formed an aluminum oxide scale, and the oxidation weight gain rate was high. Due to the presence of alumina, the contact surface between oxygen and the coating gradually decreased, and the alumina scale gradually stabilized, so the oxidation weight gain curve tended to be flat. As shown in <xref ref-type="fig" rid="F2">Figure 2B</xref>, during the 50-h oxidation, the oxidation processes of both coatings can be divided into two stages: In the initial stage (&#x3c;3&#xa0;h), the parabolic oxidation rate constant (Kp<sup>I</sup>) of the Al<sub>2</sub>O<sub>3</sub> film&#x2013;covered Ni<sub>2</sub>Al<sub>3</sub> coating is 3.2 &#xd7; 10<sup>&#x2013;13</sup>&#xa0;g<sup>2</sup>/cm<sup>4</sup>s lower than that of the naked coating with parabolic oxidation rate constant Kp<sup>I</sup> of &#x223c;4.4 &#xd7; 10<sup>&#x2013;13</sup>&#xa0;g<sup>2</sup>/cm<sup>4</sup>s. In the steady stage (&#x3e;3&#xa0;h), the parabolic oxidation rate constant (Kp<sup>&#x2161;</sup>) of the Al<sub>2</sub>O<sub>3</sub> film&#x2013;covered Ni<sub>2</sub>Al<sub>3</sub> coating is 1.2 &#xd7; 10<sup>&#x2013;13</sup>&#xa0;g<sup>2</sup>/cm<sup>4</sup>s, also lower than that of the naked coating with parabolic oxidation rate constant Kp<sup>&#x2161;</sup> of &#x223c;2.4 &#xd7; 10<sup>&#x2013;13</sup>&#xa0;g<sup>2</sup>/cm<sup>4</sup>&#xa0;s.</p>
<fig id="F2" position="float">
<label>FIGURE 2</label>
<caption>
<p>
<bold>(A)</bold> Oxidation kinetics curves and <bold>(B)</bold> corresponding parabolic plots of naked and Al<sub>2</sub>O<sub>3</sub> film&#x2013;covered Ni<sub>2</sub>Al<sub>3</sub> coatings oxidated in air at 1,000&#xa0;&#xb0;C.</p>
</caption>
<graphic xlink:href="fmats-09-934215-g002.tif"/>
</fig>
<p>The Al<sub>2</sub>O<sub>3</sub> film-covered coating macroscopic surface after oxidation is shown in <xref ref-type="fig" rid="F3">Figure 3A</xref>, and then the electrophoretic alumina film was removed using alcohol, as shown in <xref ref-type="fig" rid="F3">Figure 3B</xref>. The surface characteristics of the naked Ni<sub>2</sub>Al<sub>3</sub> coating changes with the increasing oxidation duration , as illustrated in <xref ref-type="fig" rid="F4">Figures 4A,C,E,G</xref>. Fine alumina crystals developed on the surface at the early stage of high-temperature oxidation (30&#xa0;min), and the color depth difference was caused by the distinct growth directions. The size of thin needle-like alumina crystals grew bigger after 2&#xa0;h oxidation, and the oxide scale got thicker and denser. After being oxidized for 5&#xa0;h, some acicular alumina became stagnant, cracks appeared on the surface, and the acicular alumina crystals were rapidly regenerated in the spalling area. After 50&#xa0;h of oxidation, the oxide scale is mostly composed of acicular alumina and round alumina. According to the above morphologies and the characteristics of the alumina phase structure (<xref ref-type="bibr" rid="B16">Swadba et al., 2011</xref>), it can be judged that &#x3b8;-Al<sub>2</sub>O<sub>3</sub> is rapidly formed in the early stage of oxidation, and then the &#x3b8; phase is partially converted into the &#x3b1; phase. The growth of &#x3b1;-Al<sub>2</sub>O<sub>3</sub> will inhibit the growth of the &#x3b8; phase. The lateral growth direction of &#x3b1;-Al<sub>2</sub>O<sub>3</sub> resulted in surface unevenness. The conversion of &#x3b8; phase to &#x3b1; phase will cause the microcracks or even local spalling because of volume shrinkage (the transformation from metastable alumina to &#x3b1;-Al<sub>2</sub>O<sub>3</sub> is a reconstructive phase transition, which is a first-order phase transition and the process is irreversible). The spalling area will quickly generate &#x3b8;-Al<sub>2</sub>O<sub>3</sub>, so both &#x3b8;-Al<sub>2</sub>O<sub>3</sub> and &#x3b1;-Al<sub>2</sub>O<sub>3</sub> phases can be seen on the surface after high-temperature oxidation for 50&#xa0;h. For the Al<sub>2</sub>O<sub>3</sub> film&#x2013;covered Ni<sub>2</sub>Al<sub>3</sub> coating, an &#x3b1;-Al<sub>2</sub>O<sub>3</sub> scale was formed rapidly in the early stage of oxidation. With the prolongation of oxidation time, the oxide scale gradually thickens and becomes flat (<xref ref-type="fig" rid="F4">Figures 4B,D,F,H</xref>). After 5&#xa0;h of oxidation, the scale appeared to slightly peel. After 50&#xa0;h of oxidation, a dense and stable alumina scale has been formed. Therefore, there is no phase change in the oxide scale of the Al<sub>2</sub>O<sub>3</sub> film&#x2013;covered coating during the whole oxidation process. It can be seen in <xref ref-type="fig" rid="F5">Figure 5A</xref> that the coating degradation completely conforms to the mechanism of the nickel&#x2013;aluminum coating: &#x3b4;-Ni<sub>2</sub>Al<sub>3</sub>&#x2192;&#x3b2;-NiAl&#x2192;&#x3b3;&#x2032;-Ni<sub>3</sub>Al. At the beginning of oxidation, the generated alumina is too thin and its X-ray diffraction peak intensity is weak, so the original diffraction peak pattern is partially enlarged as shown in <xref ref-type="fig" rid="F5">Figures 5B&#x2032;,C&#x2032;</xref>, from which it is known that the &#x3b1; phase is formed on the surface of the electrophoretic alumina film sample from the beginning of oxidation. Based on the XRD, SEM, and TGA analysis, the early oxidation progress of aluminide in the absence and presence of the surface Al<sub>2</sub>O<sub>3</sub> film is shown in <xref ref-type="fig" rid="F6">Figure 6</xref>. At the beginning of oxidation (Stage &#x2160;), &#x3b8;-Al<sub>2</sub>O<sub>3</sub> is rapidly formed on the naked aluminide surface, while &#x3b1;-Al<sub>2</sub>O<sub>3</sub> is formed on the surface of the aluminide coating with electrophoretic Al<sub>2</sub>O<sub>3</sub> particles (<xref ref-type="bibr" rid="B2">An et al., 2000</xref>). Then both increase to form an alumina scale (Stage &#x2161;); the alumina is much denser as shown in <xref ref-type="fig" rid="F4">Figures 4C,D</xref>. In stage &#x2162;, generated &#x3b1;-Al<sub>2</sub>O<sub>3</sub> grows inward and outward at the same time, during which the most electrophoresed Al<sub>2</sub>O<sub>3</sub> film on the surface is pushed outward, and a small part is wrapped by the outwardly growing &#x3b1;-Al<sub>2</sub>O<sub>3</sub> (<xref ref-type="bibr" rid="B8">Huang and Peng, 2016</xref>). At this time, the exposed &#x3b8;-Al<sub>2</sub>O<sub>3</sub> of the naked sample transforms into &#x3b1;-Al<sub>2</sub>O<sub>3</sub> (<xref ref-type="fig" rid="F4">Figure 4E</xref>). With &#x3b1;-Al<sub>2</sub>O<sub>3</sub> gradually increasing, an &#x3b1;-Al<sub>2</sub>O<sub>3</sub> scale was formed at the interface between NiAl coating and &#x3b8;-Al<sub>2</sub>O<sub>3</sub> (Stage &#x2163;). During this phase transition, volume shrinkage will occur, resulting in cracks or even peeling of the scale (<xref ref-type="bibr" rid="B17">Tolpygo and Clarke, 2000</xref>), which are visible on the surface topography (<xref ref-type="fig" rid="F4">Figure 4</xref>).</p>
<fig id="F3" position="float">
<label>FIGURE 3</label>
<caption>
<p>Surface with <bold>(A)</bold> alumina particles after oxidation and <bold>(B)</bold> removal of alumina particles after oxidation.</p>
</caption>
<graphic xlink:href="fmats-09-934215-g003.tif"/>
</fig>
<fig id="F4" position="float">
<label>FIGURE 4</label>
<caption>
<p>Surface morphologies of the alumina scale formed on the &#x3b4;-Ni<sub>2</sub>Al<sub>3</sub> coating at 1,000&#xb0;C for different oxidation times. <bold>(A)</bold>, <bold>(C)</bold>, <bold>(E)</bold>, and <bold>(G)</bold>: Ni<sub>2</sub>Al<sub>3</sub>; <bold>(B)</bold>, <bold>(D)</bold>, <bold>(F)</bold>, and <bold>(H)</bold>: Al<sub>2</sub>O<sub>3</sub> film&#x2013;covered Ni<sub>2</sub>Al<sub>3</sub>.</p>
</caption>
<graphic xlink:href="fmats-09-934215-g004.tif"/>
</fig>
<fig id="F5" position="float">
<label>FIGURE 5</label>
<caption>
<p>XRD patterns of <bold>(A)</bold> Ni<sub>2</sub>Al<sub>3</sub> coating at different times and <bold>(B)</bold> and <bold>(C)</bold> 30&#xa0;min and 50&#xa0;h naked and the Al<sub>2</sub>O<sub>3</sub> film&#x2013;covered Ni<sub>2</sub>Al<sub>3</sub> coating after oxidation in the air at 1,000&#xb0;C and <bold>(B&#x2032;) (C&#x2032;)</bold> locally magnified.</p>
</caption>
<graphic xlink:href="fmats-09-934215-g005.tif"/>
</fig>
<fig id="F6" position="float">
<label>FIGURE 6</label>
<caption>
<p>Schematic transient oxidation progress of the Ni<sub>2</sub>Al<sub>3</sub> coatings <bold>(A)</bold> without and <bold>(B)</bold> with the surface Al<sub>2</sub>O<sub>3</sub> particles.</p>
</caption>
<graphic xlink:href="fmats-09-934215-g006.tif"/>
</fig>
<p>The nickel aluminide thermally grows &#x3b8;-Al<sub>2</sub>O<sub>3</sub> before &#x3b1;-Al<sub>2</sub>O<sub>3</sub> because the former has lower surface energies and thus a much lower nucleation barrier &#x394;G&#x2a;. This is the direct origin of why the metastable alumina phases rather than the most stable ones usually form during the initial oxidation of &#x3b2;-NiAl (<xref ref-type="bibr" rid="B7">Huang et al., 2019</xref>). Therefore, during the subsequent oxidation, the undesirable metastable-to-stable phase transformation of alumina becomes unavoidable. The direct &#x3b1;-Al<sub>2</sub>O<sub>3</sub> formation without metastable-to-stable alumina phase transformation on typical oxide particles (e.g., &#x3b1;-Al<sub>2</sub>O<sub>3</sub>, Cr<sub>2</sub>O<sub>3</sub>, and Fe<sub>2</sub>O<sub>3</sub>) means that the template effect of the oxides isostructural to &#x3b1;-Al<sub>2</sub>O<sub>3</sub> intrinsically reduces &#x394;G&#x2a; of &#x3b1;-Al<sub>2</sub>O<sub>3</sub> down to such a level in favor of its thermal nucleation (<xref ref-type="bibr" rid="B15">Pint et al., 1997</xref>; <xref ref-type="bibr" rid="B20">Wang and Zhou, 2012</xref>; <xref ref-type="bibr" rid="B24">Yin and Zhen, 2015</xref>; <xref ref-type="bibr" rid="B7">Huang et al., 2019</xref>). The template effect has been widely studied by revealing some oxides (e.g., Cr<sub>2</sub>O<sub>3</sub> and Fe<sub>2</sub>O<sub>3</sub>), which are isostructural to &#x3b1;-Al<sub>2</sub>O<sub>3</sub>, and may serve as the nucleation sites facilitating the growth of the &#x3b1;-Al<sub>2</sub>O<sub>3</sub> (<xref ref-type="bibr" rid="B15">Pint et al., 1997</xref>; <xref ref-type="bibr" rid="B20">Wang and Zhou, 2012</xref>; <xref ref-type="bibr" rid="B24">Yin and Zhen, 2015</xref>; <xref ref-type="bibr" rid="B7">Huang et al., 2019</xref>). This interpretation coincides well with a promoted &#x3b8;-to-&#x3b1; alumina phase transformation on &#x3b2;-NiAl when it has been embedded with the fine particles of &#x3b1;-Al<sub>2</sub>O<sub>3</sub> (<xref ref-type="bibr" rid="B18">Veal et al., 2006</xref>). The electrophoretic &#x3b1;-Al<sub>2</sub>O<sub>3</sub> particles have the same HCP crystal structure as the &#x3b1;-Al<sub>2</sub>O<sub>3</sub> grown from the coating and can act as an epitaxial growth platform for &#x3b1;-Al<sub>2</sub>O<sub>3</sub> during oxidation, reducing the nucleation energy of the latter. Therefore, when the surface is completely covered with alumina nanoparticles, the &#x3b8;-to-&#x3b1; phase transition can be skipped when the coating is oxidized at 1,000&#xb0;C, and &#x3b1;-Al<sub>2</sub>O<sub>3</sub> is directly generated.</p>
<p>The Al<sub>2</sub>O<sub>3</sub> particle pretreatment significantly decreases the oxidation rate, leading to a slower degradation rate of the nickel aluminide. As seen in the cross-sectional characteristics in <xref ref-type="fig" rid="F7">Figure 7</xref>, after 50&#xa0;h of oxidation, the phase structures of both types of coatings are NiAl &#x2b; Ni<sub>3</sub>Al phases, indicating that the unstable &#x3b4;-Ni<sub>2</sub>Al<sub>3</sub> phase degenerates into the NiAl phase at a high temperature of 1,000&#xa0;&#xb0;C, and then unceasingly degenerates into the Ni<sub>3</sub>Al phase with oxidation time prolongation. In <xref ref-type="fig" rid="F7">Figure 7</xref>, the thickness of the naked coating and the Al<sub>2</sub>O<sub>3</sub> film&#x2013;covered coating after oxidation is thicker than that before oxidation, indicating that both coatings have a certain degree of Al elements internal-diffusion during the high-temperature oxidation process. It can be seen from <xref ref-type="fig" rid="F7">Figures 7A,B</xref> that the alumina scale thickness of the naked coating is about 7.9 &#xb5;m, which is twice that of the Al<sub>2</sub>O<sub>3</sub>-scale&#x2013;covered coating (&#x223c;3.5&#xa0;&#xb5;m). This is consistent with the analysis result of the oxidation growth curve. During the oxidation process, aluminum ions moving from the inside of the coating to the coating surface meet with oxygen atoms to form an aluminum oxide scale, so there will be a &#x3b3;-Ni<sub>3</sub>Al phase formed due to the Al rapid consumption between the aluminum oxide film and the nickel&#x2013;aluminum coating. Since the naked coating needs to consume more Al elements to form the aluminum oxide scale, the thickness of the &#x3b3;-Ni<sub>3</sub>Al phase coating is significantly thicker than that of the Al<sub>2</sub>O<sub>3</sub> film&#x2013;covered coating, which is near the aluminum oxide scale. The reason for the difference in the thickness of the two coatings is that electrophoretic alumina can promote the formation of &#x3b1;-Al<sub>2</sub>O<sub>3</sub> on the coating surface, which can effectively prevent the oxygen element from entering the coating, reducing the consumption of the Ni<sub>2</sub>Al<sub>3</sub> coating. Therefore, promoting the formation of stable-phase &#x3b1;-Al<sub>2</sub>O<sub>3</sub> is an effective way to improve the high-temperature oxidation resistance and prolong the life of the coating. The large difference in coating consumption in the same sample is due to the consumption of aluminum elements again to form an aluminum oxide scale after the local scale peels off. With the prolongation of oxidation time, the cracks increase and cause local peeling of the aluminum oxide scale. The spalled area will quickly deplete the nickel&#x2013;aluminum coating to form a new aluminum oxide scale.</p>
<fig id="F7" position="float">
<label>FIGURE 7</label>
<caption>
<p>Cross-sectional morphologies of the Al<sub>2</sub>O<sub>3</sub> scales on the <bold>(A)</bold> and <bold>(B)</bold> naked Ni<sub>2</sub>Al<sub>3</sub> coating, and <bold>(C)</bold> and <bold>(D)</bold> the Al<sub>2</sub>O<sub>3</sub> film&#x2013;covered Ni<sub>2</sub>Al<sub>3</sub> after 50&#xa0;h of oxidation in the air at 1,000&#xb0;C.</p>
</caption>
<graphic xlink:href="fmats-09-934215-g007.tif"/>
</fig>
</sec>
<sec sec-type="conclusion" id="s4">
<title>Conclusion</title>
<p>The Ni<sub>2</sub>Al<sub>3</sub> coating with a thickness of 35&#xa0;&#x3bc;m was prepared on the pure Ni matrix using a chemical vapor deposition method at 750&#xb0;C &#xd7; 200&#xa0;T for 3&#xa0;h, and then the Al<sub>2</sub>O<sub>3</sub> film was made to adhere to the Ni<sub>2</sub>Al<sub>3</sub> coating surface by electrophoresis technology. Because of the lower power required to form the critical nuclei, the &#x3b8;-Al<sub>2</sub>O<sub>3</sub> formed earlier on the naked Ni<sub>2</sub>Al<sub>3</sub> coating and then undergo a &#x3b8;-to-&#x3b1; Al<sub>2</sub>O<sub>3</sub> transition process during the oxidation process at 1,000&#xa0;&#xb0;C. The electrophoretic Al<sub>2</sub>O<sub>3</sub> film adhering to Ni<sub>2</sub>Al<sub>3</sub> coating can skip this phase transition because the Al<sub>2</sub>O<sub>3</sub> film on the coating surface can provide a crystal template to promote the nucleation of &#x3b1;-Al<sub>2</sub>O<sub>3</sub> at the beginning of oxidation. The rapid nucleation of &#x3b1;-Al<sub>2</sub>O<sub>3</sub> significantly reduces the oxidation rate of NiAl coating and prevents microcracks and voids caused by phase transformation.</p>
</sec>
</body>
<back>
<sec id="s5">
<title>Data Availability Statement</title>
<p>The original contributions presented in the study are included in the article/supplementary material; further inquiries can be directed to the corresponding author.</p>
</sec>
<sec id="s6">
<title>Author Contributions</title>
<p>YF carried out experiments; XS directed the experiment and analyzed experimental results; SD analyzed experimental results.</p>
</sec>
<sec id="s7">
<title>Funding</title>
<p>The work is supported by the Graduate Innovation Special Fund Project of Nanchang Hangkong University (project Grant No. YC2021-S660).</p>
</sec>
<sec sec-type="COI-statement" id="s8">
<title>Conflict of Interest</title>
<p>The authors declare that the research was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.</p>
</sec>
<sec sec-type="disclaimer" id="s9">
<title>Publisher&#x2019;s Note</title>
<p>All claims expressed in this article are solely those of the authors and do not necessarily represent those of their affiliated organizations, or those of the publisher, the editors, and the reviewers. Any product that may be evaluated in this article, or claim that may be made by its manufacturer, is not guaranteed or endorsed by the publisher.</p>
</sec>
<ref-list>
<title>References</title>
<ref id="B2">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>An</surname>
<given-names>T. F.</given-names>
</name>
<name>
<surname>Guan</surname>
<given-names>H. R.</given-names>
</name>
<name>
<surname>Sun</surname>
<given-names>X. F.</given-names>
</name>
<name>
<surname>Hu</surname>
<given-names>Z. Q.</given-names>
</name>
</person-group> (<year>2000</year>). <article-title>Effect of the &#x3b8;&#x2013;&#x3b1;-Al<sub>2</sub>O<sub>3</sub> Transformation in Scales on the Oxidation Behavior of a Nickel-Base Superalloy with an Aluminide Diffusion Coating</article-title>. <source>Oxid. Mater.</source> <volume>54</volume>, <fpage>301</fpage>&#x2013;<lpage>316</lpage>. </citation>
</ref>
<ref id="B3">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Bouchaud</surname>
<given-names>B.</given-names>
</name>
<name>
<surname>Rannou</surname>
<given-names>B.</given-names>
</name>
<name>
<surname>Pedraza</surname>
<given-names>F.</given-names>
</name>
</person-group> (<year>2013</year>). <article-title>Slurry Aluminizing Mechanisms of Ni-Based Superalloys Incorporating an Electrosynthesized Ceria Diffusion Barrier</article-title>. <source>Mater. Chem. Phys.</source> <volume>143</volume>, <fpage>416</fpage>&#x2013;<lpage>424</lpage>. <pub-id pub-id-type="doi">10.1016/j.matchemphys.2013.09.022</pub-id> </citation>
</ref>
<ref id="B4">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Goral</surname>
<given-names>M.</given-names>
</name>
<name>
<surname>Ochal</surname>
<given-names>K.</given-names>
</name>
<name>
<surname>Kubaszek</surname>
<given-names>T.</given-names>
</name>
<name>
<surname>Drajewicz</surname>
<given-names>M.</given-names>
</name>
</person-group> (<year>2020</year>). <article-title>The Influence of Deposition Technique of Aluminide Coatings on Oxidation Resistance of Different Nickel Superalloys</article-title>. <source>Mater. Today Proc.</source> <volume>33</volume>, <fpage>1746</fpage>&#x2013;<lpage>1751</lpage>. <pub-id pub-id-type="doi">10.1016/j.matpr.2020.04.863</pub-id> </citation>
</ref>
<ref id="B5">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Goward</surname>
<given-names>G. W.</given-names>
</name>
<name>
<surname>Boone</surname>
<given-names>D. H.</given-names>
</name>
</person-group> (<year>1971</year>). <article-title>Mechanisms of Formation of Diffusion Aluminide Coatings on Nickel-Base Superalloys</article-title>. <source>Oxid. Mater.</source> <volume>3</volume>, <fpage>475</fpage>&#x2013;<lpage>495</lpage>. <pub-id pub-id-type="doi">10.1007/bf00604047</pub-id> </citation>
</ref>
<ref id="B6">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Goward</surname>
<given-names>G. W.</given-names>
</name>
</person-group> (<year>1970</year>). <article-title>Current Research on the Surface Protection of Superalloys for Gas Turbine Engines</article-title>. <source>JOM</source> <volume>22</volume>, <fpage>31</fpage>&#x2013;<lpage>39</lpage>. <pub-id pub-id-type="doi">10.1007/bf03355665</pub-id> </citation>
</ref>
<ref id="B7">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Huang</surname>
<given-names>Y.</given-names>
</name>
<name>
<surname>Peng</surname>
<given-names>X.</given-names>
</name>
<name>
<surname>Chen</surname>
<given-names>Q.</given-names>
</name>
</person-group> (<year>2019</year>). <article-title>TiO2 Nanoparticles-Assisted &#x3b1;-Al2O3 Direct Thermal Growth on Nickel Aluminide Intermetallics: Template Effect of the Oxide with the Hexagonal Oxygen Sublattice</article-title>. <source>Corros. Sci.</source> <volume>153</volume>, <fpage>109</fpage>&#x2013;<lpage>117</lpage>. <pub-id pub-id-type="doi">10.1016/j.corsci.2019.03.025</pub-id> </citation>
</ref>
<ref id="B8">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Huang</surname>
<given-names>Y.</given-names>
</name>
<name>
<surname>Peng</surname>
<given-names>X.</given-names>
</name>
</person-group> (<year>2016</year>). <article-title>The Promoted Formation of an &#x3b1;-Al 2 O 3 Scale on a Nickel Aluminide with Surface Cr 2 O 3 Particles</article-title>. <source>Corros. Sci.</source> <volume>112</volume>, <fpage>226</fpage>&#x2013;<lpage>232</lpage>. <pub-id pub-id-type="doi">10.1016/j.corsci.2016.07.029</pub-id> </citation>
</ref>
<ref id="B1">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Khana</surname>
<given-names>A.</given-names>
</name>
<name>
<surname>Huang</surname>
<given-names>Y.</given-names>
</name>
<name>
<surname>Dong</surname>
<given-names>Z.</given-names>
</name>
<name>
<surname>Peng</surname>
<given-names>X.</given-names>
</name>
</person-group> (<year>2019</year>). <article-title>Effect of Cr<sub>2</sub>O<sub>3</sub> Nanoparticle Dispersions on Oxidation Kinetics and Phase Transformation of Thermally Grown Alumina on a Nickel Aluminide Coating &#x2013; ScienceDirect</article-title>. <source>Corros. Sci.</source> <volume>150</volume>, <fpage>91</fpage>&#x2013;<lpage>99</lpage>. </citation>
</ref>
<ref id="B9">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Leng</surname>
<given-names>W.</given-names>
</name>
<name>
<surname>Pillai</surname>
<given-names>R.</given-names>
</name>
<name>
<surname>Naumenko</surname>
<given-names>D.</given-names>
</name>
<name>
<surname>Galiullin</surname>
<given-names>T.</given-names>
</name>
<name>
<surname>Quadakkers</surname>
<given-names>W. J.</given-names>
</name>
</person-group> (<year>2020</year>). <article-title>Effect of Substrate Alloy Composition on the Oxidation Behaviour and Degradation of Aluminide Coatings on Two Ni Base Superalloys</article-title>. <source>Corros. Sci.</source> <volume>167</volume>, <fpage>81</fpage>&#x2013;<lpage>99</lpage>. <pub-id pub-id-type="doi">10.1016/j.corsci.2020.108494</pub-id> </citation>
</ref>
<ref id="B10">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Liu</surname>
<given-names>G.</given-names>
</name>
<name>
<surname>Li</surname>
<given-names>M.</given-names>
</name>
<name>
<surname>Zhu</surname>
<given-names>M.</given-names>
</name>
<name>
<surname>Zhou</surname>
<given-names>Y.</given-names>
</name>
</person-group> (<year>2007</year>). <article-title>Transient of Alumina Oxide Scale on &#x3b2;-NiAl Coated on M38G Alloy at 950&#xb0;C</article-title>. <source>Intermetallics</source> <volume>15</volume>, <fpage>1285</fpage>&#x2013;<lpage>1290</lpage>. <pub-id pub-id-type="doi">10.1016/j.intermet.2007.03.010</pub-id> </citation>
</ref>
<ref id="B11">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Mollard</surname>
<given-names>M.</given-names>
</name>
<name>
<surname>Rannou</surname>
<given-names>B.</given-names>
</name>
<name>
<surname>Bouchaud</surname>
<given-names>B.</given-names>
</name>
<name>
<surname>Balmain</surname>
<given-names>J.</given-names>
</name>
<name>
<surname>Bonnet</surname>
<given-names>G.</given-names>
</name>
<name>
<surname>Pedraza</surname>
<given-names>F.</given-names>
</name>
</person-group> (<year>2013</year>). <article-title>Comparative Degradation of Nickel Aluminized by Slurry and by Pack Cementation under Isothermal Conditions</article-title>. <source>Corros. Sci.</source> <volume>66</volume>, <fpage>118</fpage>&#x2013;<lpage>124</lpage>. <pub-id pub-id-type="doi">10.1016/j.corsci.2012.09.009</pub-id> </citation>
</ref>
<ref id="B12">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Montero</surname>
<given-names>X.</given-names>
</name>
<name>
<surname>Galetz</surname>
<given-names>M. C.</given-names>
</name>
<name>
<surname>Sch&#xfc;tze</surname>
<given-names>M.</given-names>
</name>
</person-group> (<year>2013</year>). <article-title>Low-activity Aluminide Coatings for Superalloys Using a Slurry Process Free of Halide Activators and Chromates</article-title>. <source>Surf. Coatings Technol.</source> <volume>222</volume>, <fpage>9</fpage>&#x2013;<lpage>14</lpage>. <pub-id pub-id-type="doi">10.1016/j.surfcoat.2013.01.033</pub-id> </citation>
</ref>
<ref id="B13">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Nicholls</surname>
<given-names>J. R.</given-names>
</name>
</person-group> (<year>2003</year>). <article-title>Advances in Coating Design for High-Performance Gas Turbines</article-title>. <source>MRS Bull.</source> <volume>28</volume> (<issue>9</issue>), <fpage>659</fpage>&#x2013;<lpage>670</lpage>. <pub-id pub-id-type="doi">10.1557/mrs2003.194</pub-id> </citation>
</ref>
<ref id="B14">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Peng</surname>
<given-names>X.</given-names>
</name>
<name>
<surname>Clarke</surname>
<given-names>D. R.</given-names>
</name>
<name>
<surname>Wang</surname>
<given-names>F.</given-names>
</name>
</person-group> (<year>2003</year>). <article-title>Transient-alumina Transformations during the Oxidation of Magnetron-Sputtered CoCrAl Nanocrystalline Coatings</article-title>. <source>Oxid. Metals</source> <volume>60</volume>, <fpage>225</fpage>&#x2013;<lpage>240</lpage>. <pub-id pub-id-type="doi">10.1023/a:1026015101783</pub-id> </citation>
</ref>
<ref id="B15">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Pint</surname>
<given-names>B. A.</given-names>
</name>
<name>
<surname>Treska</surname>
<given-names>M.</given-names>
</name>
<name>
<surname>Hobbs</surname>
<given-names>L. W.</given-names>
</name>
</person-group> (<year>1997</year>). <article-title>The Effect of Various Oxide Dispersions on the Phase Composition and Morphology of Al2O3 Scales Grown on &#x3b2;-NiAl</article-title>. <source>Oxid. Met.</source> <volume>47</volume>, <fpage>1</fpage>&#x2013;<lpage>20</lpage>. <pub-id pub-id-type="doi">10.1007/bf01682369</pub-id> </citation>
</ref>
<ref id="B16">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Swadba</surname>
<given-names>L.</given-names>
</name>
<name>
<surname>Nawrat</surname>
<given-names>G.</given-names>
</name>
<name>
<surname>Mendala</surname>
<given-names>B.</given-names>
</name>
<name>
<surname>Goral</surname>
<given-names>M.</given-names>
</name>
</person-group> (<year>2011</year>). <article-title>The Influence of Deposition Process on Structure of Platinum-Modified Aluminide Coatings O Ni-Base Superalloy</article-title>. <source>Key Eng. Mat.</source> <volume>465</volume>, <fpage>247</fpage>&#x2013;<lpage>250</lpage>. </citation>
</ref>
<ref id="B17">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Tolpygo</surname>
<given-names>V. K.</given-names>
</name>
<name>
<surname>Clarke</surname>
<given-names>D. R.</given-names>
</name>
</person-group> (<year>2000</year>). <article-title>Microstructural Study of the Theta-Alpha Transformation in Alumina Scales Formed on Nickel-Aluminides</article-title>. <source>Mater. A. T. High. Temp.</source> <volume>17</volume>, <fpage>59</fpage>&#x2013;<lpage>70</lpage>. <pub-id pub-id-type="doi">10.1179/mht.2000.011</pub-id> </citation>
</ref>
<ref id="B18">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Veal</surname>
<given-names>B. W.</given-names>
</name>
<name>
<surname>Paulikas</surname>
<given-names>A. P.</given-names>
</name>
<name>
<surname>Birtcher</surname>
<given-names>R. C.</given-names>
</name>
</person-group> (<year>2006</year>). <article-title>Mechanisms and Control of Phase Transition in Thermally Grown Aluminas</article-title>. <source>Appl. Phys. Lett.</source> <volume>89</volume>, <fpage>505</fpage>. <pub-id pub-id-type="doi">10.1063/1.2364124</pub-id> </citation>
</ref>
<ref id="B19">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Wang</surname>
<given-names>X.</given-names>
</name>
<name>
<surname>Peng</surname>
<given-names>X.</given-names>
</name>
<name>
<surname>Tan</surname>
<given-names>X.</given-names>
</name>
<name>
<surname>Wang</surname>
<given-names>F.</given-names>
</name>
</person-group> (<year>2016</year>). <article-title>The Reactive Element Effect of Ceria Particle Dispersion on Alumina Growth: A Model Based on Microstructural Observations</article-title>. <source>Sci. Rep.</source> <volume>6</volume>, <comment>29593</comment>, <fpage>1</fpage>&#x2013;<lpage>10</lpage>. <pub-id pub-id-type="doi">10.1038/srep29593</pub-id> </citation>
</ref>
<ref id="B20">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Wang</surname>
<given-names>Y. D.</given-names>
</name>
<name>
<surname>Zhou</surname>
<given-names>Y. B.</given-names>
</name>
</person-group> (<year>2012</year>). <article-title>Cyclic-Oxidation of RexOy-Modified Aluminide Coating</article-title>. <source>Amr</source> <volume>557-559</volume>, <fpage>1721</fpage>&#x2013;<lpage>1726</lpage>. <pub-id pub-id-type="doi">10.4028/www.scientific.net/amr.557-559.1721</pub-id> </citation>
</ref>
<ref id="B21">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Warnes</surname>
<given-names>B. M.</given-names>
</name>
<name>
<surname>Punola</surname>
<given-names>D. C.</given-names>
</name>
</person-group> (<year>1997</year>). <article-title>Clean Diffusion Coatings by Chemical Vapor Deposition</article-title>. <source>Surf. Coatings Technol.</source> <volume>94-95</volume>, <fpage>1</fpage>&#x2013;<lpage>6</lpage>. <pub-id pub-id-type="doi">10.1016/s0257-8972(97)00467-2</pub-id> </citation>
</ref>
<ref id="B22">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Xu</surname>
<given-names>C.</given-names>
</name>
<name>
<surname>Peng</surname>
<given-names>X.</given-names>
</name>
<name>
<surname>Wang</surname>
<given-names>F.</given-names>
</name>
</person-group> (<year>2010</year>). <article-title>Cyclic Oxidation of an Ultrafine-Grained and CeO2-Dispersed &#x3b4;-Ni2Al3 Coating</article-title>. <source>Corros. Sci.</source> <volume>52</volume>, <fpage>740</fpage>&#x2013;<lpage>747</lpage>. <pub-id pub-id-type="doi">10.1016/j.corsci.2009.10.034</pub-id> </citation>
</ref>
<ref id="B23">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Yavorska</surname>
<given-names>M.</given-names>
</name>
<name>
<surname>Sieniawski</surname>
<given-names>J.</given-names>
</name>
<name>
<surname>Filip</surname>
<given-names>R.</given-names>
</name>
<name>
<surname>Gancarczyk</surname>
<given-names>T.</given-names>
</name>
</person-group> (<year>2011</year>). <article-title>Microstructure Investigation of Aluminide Coatings after Platinum Modification Deposited by CVD Method on Inconel 713 LC Ni-Base Superalloy</article-title>. <source>Amr</source> <volume>409</volume>, <fpage>883</fpage>&#x2013;<lpage>888</lpage>. <pub-id pub-id-type="doi">10.4028/www.scientific.net/amr.409.883</pub-id> </citation>
</ref>
<ref id="B24">
<citation citation-type="journal">
<person-group person-group-type="author">
<name>
<surname>Yin</surname>
<given-names>Q. F.</given-names>
</name>
<name>
<surname>Zhen</surname>
<given-names>R.</given-names>
</name>
</person-group> (<year>2015</year>). <article-title>Effect of Y<sub>2</sub>O<sub>3</sub> on Microstructure and Oxidation Resistance Behavior of Aluminide Coating on Ni-Based Superalloy</article-title>. <source>Adv. Mat. Res.</source> <volume>13</volume>, <fpage>603</fpage>&#x2013;<lpage>607</lpage>. </citation>
</ref>
</ref-list>
</back>
</article>