Abstract
Detecting hydrogen at low concentration is essential for the early identification of leaks in hydrogen storage and transportation systems, thereby improving operational safety. In this work, thin films of tungsten trioxide (WO3), a well-known hydrogen-sensing material, were deposited via DC reactive magnetron sputtering under systematically varied gas environments to elucidate the role of deposition conditions in tailoring film morphology and sensing performance. Introducing mixed Ar/O2, Ar/He/O2, and He/O2 sputtering atmospheres with varying gas flow rates at a substrate temperature of 400 °C produced a marked reduction in grain size and film thickness compared with films grown in an equal flow-rate Ar/O2 plasma. The film synthesized in the Ar/O2 environment exhibited superior resistance modulation upon H2 exposure and significantly enhanced sensitivity compared with the other films. Gas sensing characteristics toward H2 were evaluated at operating temperatures of 100, 150, and 200 °C, and the optimized film was further investigated for low H2 concentrations down to 25 ppm. These findings demonstrate a strong correlation between microstructure and sensing response and highlight the critical influence of the deposition environment on the morphological and electronic properties of WO3 thin films, providing a viable strategy for developing next-generation high-performance hydrogen gas sensors.
1 Introduction
Amid the global energy crisis and the urgent demand for sustainable energy solutions, hydrogen (H2) has emerged as one of the most promising clean energy carriers of the 21st century owing to its high gravimetric energy density, carbon-free combustion, and compatibility with renewable energy resources (). Hydrogen plays a pivotal role in the emerging hydrogen economy, where it serves as a key medium for energy conversion, long-term energy storage, and transportation (). It is extensively utilized in proton exchange membrane fuel cells (PEMFCs) (), solid oxide fuel cells (SOFCs), power-to-hydrogen technologies, industrial manufacturing, hydrogenation processes, petroleum refining, chemical synthesis, and aerospace propulsion (; ). The integration of hydrogen into next-generation energy systems is therefore considered indispensable for achieving carbon neutrality and reducing dependence on fossil fuels.
Despite these significant advantages, the widespread deployment of hydrogen-based energy conversion and storage technologies is hindered by critical safety concerns associated with hydrogen leakage (; ). Hydrogen possesses a high combustion rate and an extremely low ignition energy (0.017 mJ), making it highly susceptible to ignition and explosion even under minor leakage conditions. Moreover, hydrogen concentrations exceeding 4,000 ppm in air fall within its flammability range and can rapidly lead to fire or explosion hazards (; ). In addition, hydrogen is the smallest and lightest molecular gas, enabling it to readily diffuse through microscopic defects and escape from storage vessels, pipelines, valves, and fuel-cell systems. Its colorless, odorless, and tasteless nature further makes leakage impossible to detect by human senses (; ).
Therefore, reliable hydrogen gas sensing has become a fundamental requirement for the safe operation of hydrogen production, storage, transportation, and utilization infrastructure. High-performance hydrogen sensors enable continuous real-time monitoring of leaks, provide early warning before hydrogen reaches its lower explosive limit, and facilitate the implementation of automatic safety measures such as system shutdown, ventilation, and leak isolation (). Furthermore, accurate hydrogen detection enhances the operational reliability and lifetime of fuel-cell systems, hydrogen refueling stations, storage tanks, and pipelines, thereby minimizing safety risks and preventing catastrophic failures (; ). Consequently, the development of highly sensitive, selective, rapid-response, and low-power hydrogen gas sensors is not only essential for ensuring public and industrial safety but also represents a critical enabling technology for the commercialization and widespread adoption of hydrogen-based energy conversion and storage systems within the emerging hydrogen economy (; ; ; ). The MOS-based sensors utilize materials whose resistance changes upon exposure to reducing or oxidizing gases (). During last 10 years, various MOS for the precise detection of reducing and oxidizing gases, materials including TiO2, SnO2, ZnO, NiO, and WO3 have been thoroughly developed (; ; ; ; ; ). Among the various MOS materials, WO3, is an n-type semiconductor with a broad band gap of 2.6–3.2 eV, that has attracted a lot of research interest due to its superior gas sensing capabilities, high chemical and thermal stability, crystallinity and surface morphology that are easily attained by a variety of physical and chemical synthesis methods (; ; ; ; ). For example, Ramya developed WO3-x thin films deposited under 10% partial pressure of O2 via RF magnetron reactive sputtering, followed by annealing at 800 °C. The films show a sensor response of maximum value 3.4% towards 100 ppm H2 at R.T., which was attributed to their high crystallinity, enhanced porosity, and increased oxygen vacancy concentration. In a connected study, developed using impulsive magnetron sputtering WO3 thin films and evaluated them for H2 sensing at concentrations of 1,000 ppm and 25 ppm at a working temperature of 150 °C. The films demonstrated response and recovery times of 210 s and 150 s for 1,000 ppm, and 510 s and 300 s for 25 ppm, respectively. To further enhance the sensitivity of WO3 towards H2, fabricated a nanoporous WO3 film using RF sputtering and coated it with a Palladium layer via e-beam evaporation. The sensor exhibited a response of 0.9 at 50 °C. In another study, to improve the sensitivity of WO3, fabricated WO3 nanorods decorated with platinum (Pt) nanoparticles using a combination of RF sputtering and the Glancing Angle Deposition (GLAD) technique. Standard DC magnetron sputtering was used to decorate Pt nanoparticles on WO3 nanorods, with deposition times ranging from 2.5 to 15 s. At 200 °C, the resulting Pt-WO3 nanorod sensors showed an ultrahigh H2 response, ranging from 1,530 to 214,000 for 150 to 3,000 ppm of H2, respectively. As discussed earlier, WO3 operates as a chemi-resistive type gas sensor, in which the electrical resistance varies when the target gas interacts with chemisorbed oxygen ions on the surface. Consequently, the surface morphology and microstructure of WO3 play a crucial role in determining its gas sensing performance (). By adjusting process parameters such as substrate temperature, sputtering pressure, and the composition of reactive gases, WO3 films can be engineered with tailored grain sizes, defect concentrations, and preferred crystallographic orientations (). These microstructural modifications directly influence gas adsorption, charge transfer, and ultimately the selectivity and sensitivity of the sensor (). Therefore, in this article, we systematically investigate how the composition of reactive gases influences the surface morphology and microstructure of WO3 thin films. By correlating these structural modifications with their corresponding gas sensing characteristics, we aim to provide deeper insight into the optimization of WO3-based resistive gas sensors.
To the best of our knowledge, the synthesis of WO3 thin films by reactive magnetron sputtering, with a specific focus on correlating varied gas composition, surface morphology, crystallinity, and crystallite size with gas-sensing performance, has not been previously reported. In this study, WO3 thin films were deposited under three sputtering atmospheres: (Ar + O2), (Ar + He + O2), and (He + O2). X-ray diffraction (XRD), X-ray photoelectron spectroscopy (XPS), UV-Visible spectroscopy, and scanning electron microscopy (SEM) were used to systematically characterize the films’ structural, morphological, and optical features. The gas sensing performance of the WO3 thin films toward 100 ppm H2 was initially investigated at operating temperatures of 100, 150, and 200 °C to determine the optimum sensing temperature. Furthermore, the sensor selectivity was evaluated against 100 ppm CO, CO2, and CH4 at the optimized operating temperature of 150 °C. The optimized WO3 thin film was further evaluated at H2 concentrations down to 25 ppm to demonstrate its suitability for early hydrogen leak detection in hydrogen energy systems.
2 Materials and methods
2.1 Synthesis of WO3 thin films
Testbourne Ltd., United Kingdom, WO3 thin films were created on ITO-coated glass and Si (100) substrates. The deposition was conducted using a DC reactive magnetron sputtering equipment (Excel Instrument, India). Before loading the sample onto the rotating substrate holder, the substrates were ultrasonically cleaned in acetone each for 10 min to remove any surface contamination and then allowed to dry naturally. A rotary pump and a turbomolecular pump (Pfeiffer Vacuum, Germany) were used to achieve a base pressure of less than 1.5 × 10−6 Torr. A mass flow controller (Alicat Scientific, United States of America) was used to deliver high-purity gases, argon (Ar), helium (He), and oxygen (O2) (99.999%), into the deposition chamber at the flow rates listed in Table 1 for each deposition. To remove any surface contamination, the target surface was sputtered for ten minutes prior to deposition. Each deposition was subsequently performed for 60 min using a 100 W (DC power supply) applied to the tungsten target, while maintaining a constant substrate temperature of 400 °C and a sputtering pressure of 2 × 10−2 Torr. To ensure the reproducibility of the deposition process, the films were deposited three times under identical experimental conditions. The repeated depositions showed consistent film characteristics, confirming the reproducibility of the deposition process. The process flow of experiments is illustrated in Figure 1.
TABLE 1
| Sample names | Gas flow rate (sccm) | Crystallite size (nm) | ||
|---|---|---|---|---|
| Ar | He | O2 | ||
| W1 | 15 | 0 | 15 | 9.23 |
| W2 | 10 | 5 | 2.96 | |
| W3 | 0 | 15 | 2.57 | |
Gas flow rate for the deposition and Crystallite size obtained using XRD data.
FIGURE 1
2.2 Characterizations
Grazing Incidence X-ray Diffraction (GIXRD) on a Malvern Panalytical Empyrean-3 (Netherlands) system was used to examine the phase structure and crystallographic characteristics of the WO3 thin films. Cu Kα radiation (λ = 0.154 nm) was used to perform the measurement at room temperature. With a step size of 0.04° and a fixed incidence angle of 1°, diffraction patterns were recorded over a 2θ range of (15–75)o. The valence states of the elements were examined through XPS (thermoscientific ESCALAB QXi). All spectra were acquired using a monochromatic Al Kα (1,486.6 eV) source with a pass energy of 20 eV for the high-resolution regions and 100 eV for the survey scan, at a base pressure of 2 × 10−9 mbar. The binding-energy scale was calibrated to the adventitious C 1s peak at 284.8 eV. Peak fitting was carried out in CasaXPS software using a Tougaard background applied over 33–41 eV for the W 4f region and 526,536 eV for the O 1s region, with component peaks modelled using a mixed Gaussian-Lorentzian line shape GL (30). The surface morphology and cross-sectional features of the WO3 thin films were observed using a FESEM (TESCAN MIRA II LMH). Additionally, the surface topography of the deposited films was characterized using an atomic force microscope (AFM; Nanosurf Naio AFM, Switzerland). The surface roughness (Sa) values were determined. The optical characteristics were examined using UV-Visible spectroscopy (HITACHI U-3300), in 200–800 nm wavelength range.
2.3 Gas sensing measurements
Gas sensing measurements of fabricated thin films of WO3 were carried out in a static, computer-controlled gas sensing instrument consists of a stainless-steel sealed chamber with openings with ports of gas inlet and outlet (Excel Instruments, India). A two-stage rotary vacuum pump was used to empty the sensor chamber prior to each measurement cycle. For electrical response measurements, silver paste was applied near the edges of the thin films (1 cm × 1 cm), serving as electrodes for the device. The films were affixed to a temperature-regulated heating stage to study the effect of operating temperature. All films were tested for their response to 100 ppm H2 gas, with the temperature varied from 100 °C to 200 °C in step of 50 °C. The electrical resistance of the films was monitored in real time for this investigation using a Keithley-2450 Source Meter that was set up in a four-probe configuration and connected to a data gathering system. Before each measurement, the desired concentrations of H2, CH4, CO2, and CO gases were prepared in the dilution chamber using 500 ppm nitrogen-balanced gas canisters for each gas, further diluted with zero air. For this study, all the gas canisters were purchased from Adhul Marketo India Private Limited. A mass flow controller was used to inject the test gas at a flow rate of 100 sccm after the baseline resistance in air had been established. The resistance of the films was continuously recorded during both gas exposure and removal. It was observed that the chamber pressure was 4 mbar during gas exposure and decreased to 0.018 mbar in the absence of gas. To evaluate each film’s gas reaction, recovery behavior, and repeatability under the same operating conditions, the process was repeated for each film. The sensitivity (S%) of WO3 thin films was calculated for reducing gases by using Equation 1 and for oxidizing gases by Equation 2 ().where is the resistance in the presence of the target gas and is the resistance in the presence of air.
3 Results and discussion
3.1 Structural analysis
Figure 2 illustrates the GIXRD patterns of WO3 thin films of all types deposited on Si (100) substrate at 400 °C. The results reveal that the films exhibit a crystalline nature, which can be attributed to the elevated substrate temperature. At this temperature, atoms have more surface mobility, which promotes nucleation and grain growth, leading to a crystalline structure. The well-defined XRD peaks were observed at 2θ values of 23.10°, 33.24°, and 54.73°, corresponding to the (020), (202), and (420) planes, respectively, in all the synthesized films. According to JCPDS card No. 43–1,035, the observed diffraction peaks confirm that the WO3 thin films exhibit a polycrystalline monoclinic phase (). It is also observed that no peaks other than those of WO3 appear in the diffraction pattern, confirming the absence of impurities in the films. A sharp diffraction peak along the (020) orientation observed in the film deposited in (Ar, O2) indicates higher crystallinity. This enhanced crystallinity can be attributed to the synergistic effect of Argon and Oxygen in the sputtering environment, where Argon facilitates efficient sputtering and the generation of energetic species, while Oxygen ensures proper oxidation, together creating favorable conditions for crystalline growth. The films deposited in (Ar, He, O2) and (He, O2) atmospheres, exhibited low crystallinity. This can be attributed to the fact that helium, being much lighter than argon, transfers very little momentum to the W target during sputtering. As a result, the sputtering yield is significantly reduced, and the adatoms arriving at the substrate surface possess insufficient mobility to facilitate ordered crystal growth (). A minor shift of the diffraction peak at 2θ = 23.10° toward higher 2θ values is observed for the film W2 and W3 indicating a decrease in interplanar spacing. Furthermore, the full width at half maximum (FWHM) of the main diffraction peak increases from 0.8209° for W1 to 2.9048° for W2 and 3.0727° for W3, indicating progressive peak broadening. The increase in FWHM suggests a decrease in crystallite size for the W2 and W3 samples compared with the W1 sample, along with an increase in structural disorder. The crystallite sizes of all samples mentioned in Table 1 for the (020) plane were calculated using the Debye-Scherrer equation (Equation 3) ().Where λ is the wavelength of the X-ray, β is the full-width at half-maximum, and θ is the diffraction angle.
FIGURE 2
3.2 UV- visible spectroscopy and indirect optical band gap
Figure 3a shows the optical properties of WO3 thin films that were studied in absorbance mode. It can be seen that the absorbance of samples W1 is lower compared to that of W2 and W3. As per the Beer-Lambert law, the absorbance is linearly dependent on the optical path length (or the material’s thickness). The optical band gap of WO3 thin films was determined using absorption spectra and photon energy, analyzed through Tauc’s plot (Equation 4).Here, α denotes the absorption coefficient, hν represents the photon energy, n denotes the types of the electronic transition (e.g., n = 1/2 for direct permitted transitions and n = 2 for indirect transition), A is the proportionality constant, and corresponds to the optical band gap energy.
FIGURE 3
Monoclinic WO3 is an indirect-gap semiconductor in which the valence-band maximum and the conduction-band minimum occur at different momentum points within the Brillouin zone, and the XRD results confirm that all the present films crystallize in the monoclinic WO3 phase (). The indirect formulation is therefore applied consistently to all three samples.
The quantity (αhν)1/2 was plotted against hν and the linear region immediately above the absorption edge was extrapolated to the energy axis. The fitting ranges were (3.29–3.56) eV for W1, (3.51–3.79) eV for W2 and (3.63–3.90) eV for W3, chosen as the widest intervals over which (αhν)1/2 varies linearly with photon energy; the corresponding correlation coefficients were R2 ≥ [0.99]. These regions are shown as bold segments in Figure 3b, and the extrapolated intercepts are marked on the energy axis.
The indirect optical band gaps obtained are 3.03, 3.31 and 3.15 eV for W1, W2 and W3 respectively. A finite absorption is observed below the fundamental edge, most pronounced for the helium-grown films, which is attributed to defect states associated with oxygen vacancies and structural disorder; the resulting uncertainty in the extrapolated gap is approximately ±0.1 eV (). The smallest gap is obtained for the well-crystallized W1 film, while the widening observed for W2 and W3 is consistent with their reduced crystallite size and increased structural disorder, which introduce band-tail states and shift the effective absorption edge to higher energy (; ).
3.3 XPS analysis
In order to examine the chemical states of the component elements and obtain a better understanding of the surface composition and electrical structure, the XPS spectra of the W1 sample were recorded. Figure 4a presents the survey spectra and high-resolution spectra of the W 4f, O 1s, and valence band (VB) regions along with a schematic illustration of the bands present in WO3 films ().
FIGURE 4
The high-resolution W 4f spectrum (Figure 4b) exhibits two prominent peaks centred at approximately 35.7 eV and 37.8 eV, corresponding to the W 4f7/2 and W 4f5/2 spin-orbit components, respectively. The spin-orbit splitting that was observed of ∼2.1 eV agrees well with reported values for hexavalent tungsten (W6+) in stoichiometric WO3. The absence of additional peaks associated with lower oxidation states such as W5+ or metallic tungsten indicates that tungsten predominantly exists in the fully oxidized state within the deposited films ().
The O 1s spectrum (Figure 4c) was deconvoluted into two distinct components. The major peak located at approximately 530.1 eV corresponds to lattice oxygen bonded to tungsten (W-O bonds) in the WO3 crystal structure. A second, broader component centered near 531.8 eV accounts for 44% of the total O 1s area. Surface hydroxyl groups, chemisorbed oxygen species such as O− and O2−, oxygen adjacent to vacancies, and adsorbed water or carbonaceous contamination all have reported binding energies within this range, and their individual contributions cannot be reliably separated by curve fitting alone. These act as donor defects, providing free electrons to the conduction band and significantly influencing the electronic and sensing properties of the material ().
The valence band spectrum (Figure 4d) provides insight into the electronic structure of the WO3 films. The valence band region between 4–8 eV is mainly dominated by hybridized O 2p -W 5d states, which form the upper portion of the valence band. By linearly extending the valence band’s leading edge to the baseline close to the Fermi level (Ef = 0 eV), the valence band maximum (VBM) was found. The extrapolated intercept occurs at approximately 2.87 eV, indicating that the VBM lies 2.87 eV below the Fermi level ().
By combining this VBM value with the optical band gap obtained from UV-Vis spectroscopy (∼3.03 eV), the position of the conduction band minimum (CBM) can be estimated using Equation 5 ().
This calculation places the conduction band approximately 0.16 eV above the Fermi level, confirming that the Fermi level is located close to the conduction band as shown in (Figure 4e). Such an electronic configuration is characteristic of n-type WO3, where the electron concentration is largely governed by oxygen vacancy donor states ().
3.4 Surface morphology, cross-sectional FESEM, and elemental composition
FESEM analysis (Figures 5a–c) shows that gas composition strongly controls the surface morphology of the WO3 films. The Ar + O2-grown film (W1) developed the coarsest surface nanostructures, since heavy Ar+ ions deliver high sputtering yield and adatom kinetic energy, while O2 supports stoichiometric oxide formation together favoring larger grain growth. As Ar flow was progressively replaced by He (Table 1), grain size dropped sharply and grain-boundary density rose correspondingly (Figures 5b,c), consistent with He+ ions’ weaker momentum transfer and lower adatom mobility, which promotes nucleation of many small crystallites instead of few large grains (). The three films were deposited under identical power and duration, yet the cross-sectional FESEM images in (Figures 6a–c) give thicknesses of approximately 650, 337 and 222 nm for W1, W2 and W3, corresponding to deposition rates of 10.83, 5.61 and 3.7 nm/min. This reduction follows directly from the momentum-transfer efficiency at the target: the energy-transfer factor 4M1M2/(M1+M2)2 is ≈ 0.586 for Ar-W but only ≈0.083 for He-W, so the light He ions sputter tungsten far less efficiently ().
FIGURE 5
FIGURE 6
Two mechanisms explain why the He-grown films remain poorly crystalline with smaller grains despite adequate substrate temperature (T). First, a thermal calculation rules out insufficient surface diffusion: at the deposition temperature, WO3 (Melting temperature (Tm) ≈ 1,200 °C) sits at a homologous temperature T/Tm ≈ 0.46, well above the threshold for active surface and grain-boundary diffusion, and above typical amorphous to crystalline transition temperatures. So, the limiting factor isn't thermal mobility; it's growth chemistry. Helium’s high ionization potential (24.6 eV) and long-lived 19.8 eV metastable states dissociate O2 efficiently via Penning ionization, boosting atomic oxygen flux at the substrate (). Combined with reduced W flux (from the lower sputtering yield above), this sharply raises the O: W arrival ratio. Each incoming W atom is over-oxidized before it can incorporate into the lattice, suppressing the sub-stoichiometric transient states that normally seed crystalline nucleation, producing a fully oxidized but structurally disordered network instead (). EDS (Table 2) is consistent with this picture as W content drops to 7.56 at. % and O rises to 92.44 at. % in the He-grown W3 film, reflecting the same two effects already established, namely, lower W sputtering yield from lighter He+ ions, and higher O ionization/reaction rate from greater ionization energy of He.
TABLE 2
| Sample names | Elemental composition (at. %) | Indirect band gap () | |
|---|---|---|---|
| W | O | ||
| W1 | 16.37 | 83.63 | 3.00 |
| W2 | 13.63 | 86.37 | 3.31 |
| W3 | 7.56 | 92.44 | 3.15 |
Elemental composition and indirect band gap of WO3 thin films as a function of gas flow.
Grain-size distributions were determined from representative FESEM images per sample taken from different regions, using ImageJ. At least 100–150 grains were measured per sample. The resulting grain sizes are 108 ± 33 nm for W1, 19 ± 4 nm for W2 and 24 ± 6 nm for W3, where the uncertainty is the standard deviation of the distribution. The corresponding histograms are shown in Figure 7.
FIGURE 7
The grain size of the Ar grown film is roughly five times larger than that of the films deposited in helium-containing discharges, consistent with the narrower XRD reflections and the higher surface roughness of W1 (Sa ∼ 2.5 nm, compared with 0.3 and 0.8 nm calculated from AFM images as shown in Figure 8). We note that the mean sizes obtained for W2 and W3 approach the resolution limit of the FESEM measurement and should be regarded as upper estimates for these films. In all cases the FESEM grain size exceeds the crystallite size obtained from XRD line broadening (9.23, 2.96 and 2.57 nm), indicating that the observed grains are agglomerates comprising several coherently diffracting domains.
FIGURE 8
3.5 Gas sensing characteristics
For gas sensing measurements, establishing an ohmic contact between the metal and the sensing material is essential, as it minimizes interfacial resistance and ensures efficient charge transport. The nature of the metal-semiconductor interface was investigated through I-V measurements conducted over the voltage range of 2–10 V. As illustrated in Figure 9, the linear behavior of the I-V curves indicates the establishment of an ohmic contact between Ag and the WO3 thin film. Prior to gas exposure, the sensing chamber was purged with dry air, followed by the introduction of 100 ppm H2 for each measurement cycle.
FIGURE 9
Generally, the operating temperature is one of the most critical parameters affecting the gas-sensing performance, as it strongly affects the adsorption and desorption behavior of target gas molecules on the surface of the sensing material (). To determine the optimal working temperature, all samples (W1-W3) were systematically evaluated at 100, 150, and 200 °C under a constant H2 concentration of 100 ppm. The results presented in Figure 10a show a clear temperature-dependent variation in the sensitivity of deposited films. The W1 film exhibited a gradual increase in sensitivity, reaching a maximum of ∼86.18% at 150 °C, followed by a decline at higher temperatures.
FIGURE 10
In contrast, W2 demonstrated a comparatively lower sensitivity of ∼77.89% at 150 °C. The increase in sensitivity with temperature up to 150 °C can be attributed to the enhanced reaction kinetics between H2 molecules and chemisorbed oxygen species on the WO3 surface. However, when the optimal operating temperature is exceeded, excessively high temperatures promote rapid thermal desorption of adsorbed oxygen species and gas molecules from the material surface, thereby reducing their surface residence time and the availability of active sites for interaction with H2 (). Consequently, the gas-surface interaction is reduced, leading to a deterioration in the gas sensing performance at higher temperatures. Thus, the maximum response at 150 °C can be attributed to a favorable balance between adsorption, surface reaction kinetics, and thermal desorption processes (; ; ). In contrast, W3 demonstrated least sensing performance in all temperature range that mentioned as illustrated in Figure 10a. These differences in sensing behavior are likely governed by variations in surface adsorption kinetics, defect density, and charge carrier mobility, all of which are influenced by the intrinsic composition and morphology of the materials. Collectively, the findings suggest that W1 is best suited for medium temperature sensing applications (at 150 °C), while W2 exhibits higher efficiency under elevated temperature conditions (at 200 °C), thereby underscoring the potential of temperature optimization for tailoring hydrogen sensing performance in practical applications. The improved gas sensing performance of the W1 samples can be attributed to the higher density of adsorbed oxygen ions on their surface, facilitated by the larger grain boundaries that provide additional active sites and accelerate the reaction rate with hydrogen molecules. Furthermore, the increased surface area relative to the other films promotes more efficient adsorption-desorption processes, thereby improving overall sensitivity. After optimizing the operating temperature, additional W1 films were subjected to gas sensing tests toward 100 ppm CO, CO2, and CH4 at the optimum temperature of 150 °C. The films demonstrated highest response to H2, showing a sensitivity of 86.18% with fast response and recovery times of 22 s and 108 s, respectively, thereby confirming their superior selectivity and rapid dynamic behavior toward hydrogen as illustrated in Figure 10b. As previously discussed, the W1 sample exhibited high sensitivity toward 100 ppm H2.
To further evaluate its detection limit, the film was tested at concentrations of 25, 50, 75, and 100 ppm. The results revealed good sensitivity across all concentrations, with the maximum response observed at 100 ppm H2, as shown in Figure 11a. From a practical application perspective, repeatability is a critical parameter in evaluating the reliability of gas sensor films. Figure 11b presents the dynamic response curve of the W1 sample toward 100 ppm H2 at the optimized operating temperature of 150 °C. As H2 is a reducing gas, its introduction into the sensing chamber results in a decrease in the film resistance, which is consistent with the well-established n-type semiconducting behavior of WO3. The repeatability of the sensing response was evaluated over three consecutive sensing cycles under identical experimental conditions. The sensitivities obtained in the three cycles were 86.93%, 86.18%, and 88.40%, corresponding to an average sensitivity of 87.17% ± 1.13%. The small variation in sensitivity demonstrates the good repeatability and stability of the W1 sensor toward H2. The n-type semiconducting behavior of WO3 was also confirmed from XPS data analysis as mentioned in the above Section 3.3. Notably, the response curves exhibit consistent maximum amplitudes across multiple cycles, demonstrating excellent repeatability of the sensing performance. In Table 3, the hydrogen gas sensing performance of WO3 thin films synthesized by different fabrication techniques, such as RF magnetron sputtering, hydrothermal synthesis, and solvent-calcination assisted synthesis, was systematically compared. The study revealed that the gas-sensing properties of WO3 thin films are strongly influenced by both the operating temperature and the surface morphology. Specifically, variations in synthesis methods lead to differences in grain size, porosity, surface area, and crystallinity, which in turn affect the adsorption-desorption behavior of hydrogen molecules on the film surface (). Consequently, optimizing the synthesis technique and operating temperature is crucial to achieving high sensitivity and fast response-recovery characteristics.
FIGURE 11
TABLE 3
| Materials | Synthesis technique | Working temperature (oC) | Conc. of H2 (ppm) | Sensitivity (%) | Response time (s) | Recovery time (s) | Ref. |
|---|---|---|---|---|---|---|---|
| WO3 | RF sputtering | 30 | 100 | 3.24 | 1.6 | 2.8 | () |
| DC sputtering | 300 | 100 | 99.5 | - | - | () | |
| Hydrothermal | 100 | 75 | 78 | 189.82 | 201.32 | () | |
| Hydrothermal | 250 | 5,000 | 70 | 10–200 | 20–1,100 | () | |
| Solvent and calcination | 110 | 500 | 1.3 | 8 | 13 | () | |
| DC sputtering | 150 | 100 | 86.18 | 22 | 108 | This article |
Summary of recent developments of WO3 thin films based hydrogen gas sensors synthesized by different synthesis techniques.
3.6 Gas sensing mechanism
The gas-sensing mechanism of WO3 thin films, like other metal oxide semiconductors (MOS), relies on electrical resistance modulation brought induced by surface contacts (). Initially, oxygen molecules adsorb onto the WO3 surface when the sensor is exposed to ambient air. A depletion layer forms at the grain boundaries as a result of the chemisorbed oxygen species (, , or ) extracting electrons from the conduction band due to their high electronegativity (Figure 12a). This electron withdrawal reduces the free carrier concentration, thereby increasing the resistance of the film. The process of adsorption of atmospheric oxygen and the subsequent trapping of electrons from the sensing material are illustrated by Equations 6, 7, respectively (; ).
FIGURE 12
As shown in Figure 12b, for hydrogen as a reducing gas, H atoms react with the previously adsorbed oxygen ions (, , or ), producing water as a byproduct which results in the release of trapped electrons into the conduction band, as shown in Equation 8 (). Due to the n-type behavior of WO3, this process decreases the material’s resistance due to a decrease in charge carrier concentration and electron concentration.
4 Conclusion
The WO3 thin films were synthesized by DC reactive magnetron sputtering under varied gas environments to elucidate the influence of the deposition atmosphere on their structural, optical, morphological, and gas sensing properties. The incorporation of helium reduced the sputtering yield and adatom mobility, resulting in smaller grain sizes and thinner films. Among all samples, Ar/O2 grown film (W1) exhibited the highest sensitivity (∼86.18%) toward 100 ppm H2 at 150 °C, with rapid response and recovery times of 22 s and 108 s, respectively, together with excellent selectivity over CO, CO2, and CH4. Furthermore, the optimized W1 sensor demonstrated reliable hydrogen detection at concentrations as low as 25 ppm, highlighting its potential for early hydrogen leak detection in hydrogen storage, transportation, and fuel-cell systems. The enhanced sensing performance is attributed to the optimized crystallinity, balanced charge depletion width, and abundant surface adsorption sites that promote efficient gas adsorption and charge transfer. These findings demonstrate that precise control of the reactive sputtering atmosphere is an effective strategy for tailoring the microstructure and charge transport characteristics of WO3 thin films, paving the way for the development of highly sensitive, reliable, and low concentration hydrogen sensors for safe hydrogen energy applications.
Statements
Data availability statement
The original contributions presented in the study are included in the article/supplementary material, further inquiries can be directed to the corresponding authors.
Author contributions
SK: Data curation, Investigation, Methodology, Writing – original draft. AK: Data curation, Formal Analysis, Resources, Validation, Visualization, Writing – review and editing. SB: Data curation, Formal Analysis, Validation, Visualization, Writing – review and editing. HY: Data curation, Formal Analysis, Software, Validation, Visualization, Writing – review and editing. AC: Formal Analysis, Methodology, Validation, Visualization, Writing – review and editing. SA: Formal Analysis, Writing – review and editing. AS: Formal Analysis, Writing – review and editing. RP: Formal Analysis, Funding acquisition, Methodology, Supervision, Validation, Writing – review and editing.
Funding
The author(s) declared that financial support was received for this work and/or its publication. The authors gratefully acknowledge UPES and the Central Instrumentation Centre for providing research facilities and financial support. SK acknowledges UPES for the award of the JRF fellowship. ASK would like to acknowledge CSIR, New Delhi for the SRF fellowship. AS also acknowledges the financial support received from ANRF (SERB) under Grant No. 2023/000242, as well as IoE FRP grants for 2023–2024 and 2025–2026.
Conflict of interest
The author(s) declared that this work was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.
Generative AI statement
The author(s) declared that generative AI was not used in the creation of this manuscript.
Any alternative text (alt text) provided alongside figures in this article has been generated by Frontiers with the support of artificial intelligence and reasonable efforts have been made to ensure accuracy, including review by the authors wherever possible. If you identify any issues, please contact us.
Publisher’s note
All claims expressed in this article are solely those of the authors and do not necessarily represent those of their affiliated organizations, or those of the publisher, the editors and the reviewers. Any product that may be evaluated in this article, or claim that may be made by its manufacturer, is not guaranteed or endorsed by the publisher.
References
1
Al-DiabatA. M.AlgadriN. A.AhmedN. M.AbuelsamenA.BidierS. A. (2021). A high-sensitivity hydrogen gas sensor based on carbon nanotubes fabricated on SiO 2 substrate. Nanocomposites7 (1), 172–183. 10.1080/20550324.2021.1977063
2
AlamriM. (2025). A review of chemoresistive hydrogen gas sensors based on low-dimensional materials. Arabian J. Sci. Eng.50 (9), 6195–6219. 10.1007/s13369-024-09770-4
3
AngelicoR.GiamettaF.BianchiB.CatalanoP. (2025). Green hydrogen for energy transition: a critical perspective. Energies18 (2), 404. 10.3390/en18020404
4
BarathyT. R.YadavP. K.MondalA.AjithaB.JarugalaJ.Kumar ReddyY. A. (2024). High porosity and oxygen vacancy enriched WO3-x thin films for room temperature hydrogen gas sensors. Int. J. Hydrogen Energy50, 878–888. 10.1016/j.ijhydene.2023.07.218
5
BellK. L.DalgarnoA.KingstonA. E. (1968). Penning ionization by metastable helium atoms. J. Phys. B Atomic Mol. Phys.1 (1), 303–322. 10.1088/0022-3700/1/1/303
6
BraultP.ThomannA.-L.CavarrocM. (2023). Theory and molecular simulations of plasma sputtering, transport and deposition processes. Eur. Phys. J. D77 (2), 19. 10.1140/epjd/s10053-023-00592-x
7
ButtnerW. J.PostM. B.BurgessR.RivkinC. (2011). An overview of hydrogen safety sensors and requirements. Int. J. Hydrogen Energy36 (3), 2462–2470. 10.1016/j.ijhydene.2010.04.176
8
Ceviz ŞakarB. (2024). H2 gas response of NiO thin film at different gas concentrations. Türk Doğa Ve Fen Derg. (1), 77–81. 10.46810/tdfd.1425425
9
ChangC.-H.ChouT. C.ChenW. C.NiuJ. S.LinK. W.ChengS. Y.et al (2020). Study of a WO3 thin film based hydrogen gas sensor decorated with platinum nanoparticles. Sensors Actuators B Chem.317, 128145. 10.1016/j.snb.2020.128145
10
ChaudhariG. N.BendeA.BodadeA.PatilS.SapkalV. (2006). Structural and gas sensing properties of nanocrystalline TiO2:WO3-based hydrogen sensors. Sensors Actuators B Chem.115 (1), 297–302. 10.1016/j.snb.2005.09.014
11
ChawlaA. K.SinghalS.GuptaH. O.ChandraR. (2008). Effect of sputtering gas on structural and optical properties of nanocrystalline tungsten oxide films. Thin Solid Films517 (3), 1042–1046. 10.1016/j.tsf.2008.06.068
12
ChawlaA. K.SinghalS.Om GuptaH.ChandraR. (2009). Influence of nitrogen doping on the sputter-deposited WO3 films. Thin Solid Films518 (5), 1430–1433. 10.1016/j.tsf.2009.09.060
13
ChenX.ZhangB.SunJ.QinC.CaoJ.WangY. (2025). Oxygen defect engineering regulation of WO3-x for low-temperature hydrogen detection. J. Alloys Compd.1039, 183329. 10.1016/j.jallcom.2025.183329
14
DingQ.WangY.GuoP.LiJ.ChenC.WangT.et al (2020). Cr-Doped urchin-like WO3 hollow spheres: the cooperative modulation of crystal growth and energy-band structure for high-sensitive acetone detection. Sensors20 (12), 3473. 10.3390/s20123473
15
DongL.JiaR.XinB.PengB.ZhangY. (2017). Effects of oxygen vacancies on the structural and optical properties of β-Ga2O3. Sci. Rep.7 (1), 40160. 10.1038/srep40160
16
DongC.ZhaoR.YaoL.RanY.ZhangX.WangY. (2020). A review on WO3 based gas sensors: morphology control and enhanced sensing properties. J. Alloys Compd.820, 153194. 10.1016/j.jallcom.2019.153194
17
DongH.-D.ZhaoJ. P.PengM. X.ZhangY. H.XuP. Y. (2023). Au-modified spindle ZnO for high efficiency H2 sensors. Vacuum207, 111597. 10.1016/j.vacuum.2022.111597
18
DwivediC.SrivastavaS.KumarA.SinghP. (2025). Role of oxygen vacancies in improving the NO gas sensing behavior of DC magnetron sputtered sub-stoichiometric WO3 thin films. Phys. Scr.100 (2), 025928. 10.1088/1402-4896/ada311
19
FedorenkoG.OleksenkoL.MaksymovychN.VasylenkoI. (2020). Cerium-doped SnO2 nanomaterials with enhanced gas-sensitive properties for adsorption semiconductor sensors intended to detect low H2 concentrations. J. Mater. Sci.55 (35), 16612–16624. 10.1007/s10853-020-05199-w
20
GaoL.TianY.HussainA.GuanY.XuG. (2024). Recent developments and challenges in resistance-based hydrogen gas sensors based on metal oxide semiconductors. Anal. Bioanal. Chem.416 (16), 3697–3715. 10.1007/s00216-024-05213-z
21
GuH.WangZ.HuY. (2012). Hydrogen gas sensors based on semiconductor oxide nanostructures. Sensors12 (5), 5517–5550. 10.3390/s120505517
22
GuptaS. P.NishadH. H.PatilV. B.ChakaneS. D.MoreM. A.LateD. J.et al (2020). Morphology and crystal structure dependent pseudocapacitor performance of hydrated WO 3 nanostructures. Mater. Adv.1 (7), 2492–2500. 10.1039/D0MA00518E
23
HanS.-I.KumarM.DuyL. T.YeasminR.ParkC.JungG.et al (2024). Effect of structural changes of Pd/WO3 thin films on response direction and rate in hydrogen detection. Sensors Actuators B Chem.404, 135259. 10.1016/j.snb.2023.135259
24
HaviarS.ČapekJ.BatkováŠ.KumarN.DvořákF.DuchoňT.et al (2018). Hydrogen gas sensing properties of WO3 sputter-deposited thin films enhanced by on-top deposited CuO nanoclusters. Int. J. Hydrogen Energy43 (50), 22756–22764. 10.1016/j.ijhydene.2018.10.127
25
HorprathumM.SrichaiyaperkT.SamransuksamerB.WisitsoraatA.EiamchaiP.LimwicheanS.et al (2014). Ultrasensitive hydrogen sensor based on Pt-Decorated WO3 nanorods prepared by glancing-angle dc magnetron sputtering. ACS Appl. Mater. and Interfaces6 (24), 22051–22060. 10.1021/am505127g
26
HwangT.-Y.GoG. M.ParkS.LeeJ.SongY.KimS.et al (2019). Pt/Graphene catalyst and tellurium nanowire-based thermochemical hydrogen (TCH) sensor operating at room temperature in wet air. ACS Appl. Mater. and Interfaces11 (50), 47015–47024. 10.1021/acsami.9b12604
27
KadhimI. H.HassanH. A.IbrahimF. T. (2020). Hydrogen gas sensing based on nanocrystalline SnO2 thin films operating at low temperatures. Int. J. Hydrogen Energy45 (46), 25599–25607. 10.1016/j.ijhydene.2020.06.136
28
Karthik YadavP. V.AjithaB.ReddyY. A. K.Minnam ReddyV. R.ReddeppaM.KimM. D. (2021). Effect of sputter pressure on UV photodetector performance of WO3 thin films. Appl. Surf. Sci.536, 147947. 10.1016/j.apsusc.2020.147947
29
KavithaV. S.Reshmi KrishnanR.Sreeja SreedharanR.SureshK.JayasankarC.Mahadevan PillaiV. (2019). Tb3+-doped WO3 thin films: a potential candidate in white light emitting devices. J. Alloys Compd.788, 429–445. 10.1016/j.jallcom.2019.02.222
30
KimJ.-H.MirzaeiA.Woo KimH.WuP.KimS. S. (2019). Design of supersensitive and selective zno-nanofiber-based sensors for H2 gas sensing by electron-beam irradiation. Sensors Actuators B Chem.293, 210–223. 10.1016/j.snb.2019.04.113
31
KimuraY.IbanoK.UehataK.HiraiI.Tae LeeH.UedaY. (2020). Improved hydrogen gas sensing performance of WO3 films with fibrous nanostructured surface. Appl. Surf. Sci.532, 147274. 10.1016/j.apsusc.2020.147274
32
KumarS.Umamaheswara RaoA.ChawlaA. K.PandeyR. K. (2025). Exploring the role of substrate temperature in tailoring the gas sensing performance of sputter-deposited WO3 films. Phys. Scr.100 (8), 085965. 10.1088/1402-4896/adf6ef
33
KumarS.RaoA. U.ChawlaA. K.AwasthiS.PandeyR. K. (2026). Exploring the role of metal oxide heterostructures for next-generation gas sensors: a focus on NH3, H2S and NO2 gases. Chem. Phys. Impact12, 100986. 10.1016/j.chphi.2025.100986
34
LiH.WuC. H.LiuY. C.YuanS. H.ChiangZ. X.ZhangS.et al (2021). Mesoporous WO3-TiO2 heterojunction for a hydrogen gas sensor. Sensors Actuators B Chem.341, 130035. 10.1016/j.snb.2021.130035
35
LuJ.LeeC. G. (2012). Numerical estimates for energy of sputtered target atoms and reflected Ar neutrals in sputter processes. Vacuum86 (8), 1134–1140. 10.1016/j.vacuum.2011.10.018
36
MazurM.KapuścikP.WeichbrodtW.DomaradzkiJ.MazurP.KotM.et al (2023). WO3 thin-film optical gas sensors based on gasochromic effect towards low hydrogen concentrations. Materials16 (10), 3831. 10.3390/ma16103831
37
MenonS. K.KumarA.MondalS. (2025). Advancements in hydrogen gas leakage detection sensor technologies and safety measures. Clean. Energy9 (1), 263–277. 10.1093/ce/zkae122
38
MensahR. A.CorreaA.Asante-OkyereS.WallmarkC.FörsthM. (2026). A comprehensive review of risks and mitigation strategies for safe hydrogen infrastructure deployment. Front. Chem. Eng.8, 1721648. 10.3389/fceng.2026.1721648
39
MineoG.MoulaeeK.NeriG.MirabellaS.BrunoE. (2021). H2 detection mechanism in chemoresistive sensor based on low-cost synthesized WO3 nanorods. Sensors Actuators B Chem.348, 130704. 10.1016/j.snb.2021.130704
40
MishraV.WarshiM. K.SatiA.KumarA.MishraV.SagdeoA.et al (2018). Diffuse reflectance spectroscopy: an effective tool to probe the defect states in wide band gap semiconducting materials. Mater. Sci. Semicond. Process.86, 151–156. 10.1016/j.mssp.2018.06.025
41
NairA. S.SK. C.AbrahamJ. E.GeorgeP.JosephC.BijuP.et al (2022). Effect of substrate temperature on the near-infrared shielding properties of WO3-x thin films deposited by RF magnetron sputtering. Vacuum202, 111143. 10.1016/j.vacuum.2022.111143
42
NasitM.VijA.KumarR.BrajpuriyaR. K.DalelaS.AlviP. A.et al (2024). Investigation of the structural and optical properties of g-C3N4/ZrO2 nanocomposites. J. Electron. Mater.53 (10), 5904–5915. 10.1007/s11664-024-11070-4
43
PerrozziF.EmamjomehS.PaolucciV.TaglieriG.OttavianoL.CantaliniC. (2017). Thermal stability of WS2 flakes and gas sensing properties of WS2/WO3 composite to H2, NH3 and NO2. Sensors Actuators B Chem.243, 812–822. 10.1016/j.snb.2016.12.069
44
RamanaC. V.UtsunomiyaS.EwingR. C.JulienC. M.BeckerU. (2006). Structural stability and phase transitions in WO3 thin films. J. Phys. Chem. B110 (21), 10430–10435. 10.1021/jp056664i
45
RaoA. U.TiwariS. K.KharbA. S.HothiN.SaxenaV.ChawlaA. K. (2025). Harnessing innovative sputtering approaches to enhance VN coatings with superior mechanical and self-lubricating properties. J. Mater. Sci.60 (18), 7429–7465. 10.1007/s10853-025-10896-5
46
RighettoniM.AmannA.PratsinisS. E. (2015). Breath analysis by nanostructured metal oxides as chemo-resistive gas sensors. Mater. Today18 (3), 163–171. 10.1016/j.mattod.2014.08.017
47
RoloI.CostaV. A. F.BritoF. P. (2023). Hydrogen-based energy systems: current technology development status, opportunities and challenges. Energies17 (1), 180. 10.3390/en17010180
48
Sáenz-HernándezR. J.Herrera-PérezG. M.Uribe-ChaviraJ. S.Grijalva-CastilloM. C.Elizalde-GalindoJ. T.Matutes-AquinoJ. A. (2022). Correlation between thickness and optical properties in nanocrystalline γ-Monoclinic WO3 thin films. Coatings12 (11), 1727. 10.3390/coatings12111727
49
SalimiM.HosseinpourM.N.BorhaniT. (2022). The role of clean hydrogen value chain in a successful energy transition of Japan. Energies15 (16), 6064. 10.3390/en15166064
50
SaruhanB.Lontio FomekongR.NahirniakS. (2021). Review: influences of semiconductor metal oxide properties on gas sensing characteristics. Front. Sensors2, 657931. 10.3389/fsens.2021.657931
51
SharmaS.AgarwalS.JainA. (2021). Significance of hydrogen as economic and environmentally friendly fuel. Energies14 (21), 7389. 10.3390/en14217389
52
SinghS.GurawalP.MalikG.KaurD.ChandraR. (2024). Temperature-dependent wetting and other physical characteristics of sputtered grown WO3 thin films. Bull. Mater. Sci.47 (3), 137. 10.1007/s12034-024-03243-y
53
StaerzA.SomacescuS.EpifaniM.KidaT.WeimarU.BarsanN. (2020). WO3 -Based gas sensors: identifying inherent qualities and understanding the sensing mechanism. ACS Sensors5 (6), 1624–1633. 10.1021/acssensors.0c00113
54
StaffellI.ScammanD.Velazquez AbadA.BalcombeP.DoddsP. E.EkinsP.et al (2019). The role of hydrogen and fuel cells in the global energy system. Energy and Environ. Sci.12 (2), 463–491. 10.1039/C8EE01157E
55
SunM.ZhangS.ZhangZ.ZhangH.WangY.JingX.et al (2021). Effect of C6H14N2O7 and reaction temperature on sensing properties of hierarchical WO3 for H2S sensor. J. Mater. Sci.56 (20), 11801–11813. 10.1007/s10853-021-06054-2
56
TajimaC.SawadaK.OkazakiS.KasaiN. (2025). Hydrogen sensing performance and stability of WO3–SiO2 composite film doped with Pt catalyst. J. Sol-Gel Sci. Technol.113 (3), 683–695. 10.1007/s10971-024-06635-y
57
VermaA. K.PrakashC.YadavN.VermaV.SinghP.OjhaS.et al (2025). Enhanced hydrogen gas sensing performance with Ag-doped WO3 thin film. Int. J. Hydrogen Energy137, 1161–1170. 10.1016/j.ijhydene.2024.08.109
58
VidišM.ShpetnyiI. O.RochT.SatrapinskyyL.PatrnčiakM.PlecenikA.et al (2021). Flexible hydrogen gas sensor based on a capacitor-like Pt/TiO2/Pt structure on polyimide foil. Int. J. Hydrogen Energy46 (36), 19217–19228. 10.1016/j.ijhydene.2021.03.052
59
VitoriaI.Ruiz ZamarreñoC.OzcarizA.MatiasI. R. (2021). Fiber optic gas sensors based on lossy mode resonances and sensing materials used therefor: a comprehensive review. Sensors21 (3), 731. 10.3390/s21030731
60
VuongN. M.TrungT. N.HienT. T.ChinhN. D.QuangN. D.LeeD.et al (2015). Ni2O3 decoration of WO3 thin film for high sensitivity NH3 gas sensor. Mater. Trans.56 (9), 1354–1357. 10.2320/matertrans.MA201572
61
WangW.JanottiA.Van de WalleC. G. (2017). Phase transformations upon doping in WO3. J. Chem. Phys.146 (21), 214504. 10.1063/1.4984581
62
WangC.LiJ.LuoC.WangX.YangM.XiongZ.et al (2025). SnO2-based resistive hydrogen gas sensor: a comprehensive review from performance to function optimization. Mater. Sci. Semicond. Process.188, 109209. 10.1016/j.mssp.2024.109209
63
WangY.LiJ.ZhangD.ZhouT.SunM.ChenS.et al (2025). Low temperature part per billion H 2 S sensor based on P–N CuO–WO 3 heterostructured microflowers. ACS Sensors10 (6), 4442–4453. 10.1021/acssensors.5c00738
64
WideraB. (2020). Renewable hydrogen implementations for combined energy storage, transportation and stationary applications. Therm. Sci. Eng. Prog.16, 100460. 10.1016/j.tsep.2019.100460
65
XueZ.JiaX.GaoX.WuY.DongZ.HuQ.et al (2023). Regulating the electronic status on open WO2.83 surfaces for ultrasensitive H2S sensors. Sensors Actuators B Chem.385, 133569. 10.1016/j.snb.2023.133569
66
ZhongA.ShenB.WangT.JinH.XieY.ZhangD.et al (2021). Ultrafast H2 gas nanosensor for ppb-level H2 gas detection based on GaN honeycomb nanonetwork. Sensors Actuators B Chem.329, 129079. 10.1016/j.snb.2020.129079
Summary
Keywords
DC reactive magnetron sputtering, fuel cells, hydrogen economy, hydrogen gas sensing, hydrogen leak detection, microstructure engineering, WO3 thin films
Citation
Kumar S, Kharb AS, Bist S, Yadav H, Chawla AK, Awasthi S, Singh A and Pandey RK (2026) Tailoring surface and structural properties of WO3 thin films via mixed-gas plasma deposition for optimized H2 gas sensing performance. Front. Mater. 13:1942932. doi: 10.3389/fmats.2026.1942932
Received
20 July 2026
Revised
09 October 2026
Accepted
12 October 2026
Published
03 November 2026
Volume
13 - 2026
Edited by
Indu Sharma, Chung-Ang University, Republic of Korea
Reviewed by
Reza Zarei Moghadam, Arak University, Iran
Roshini Xavier, Vellore Institute of Technology, India
Updates
Copyright
© 2026 Kumar, Kharb, Bist, Yadav, Chawla, Awasthi, Singh and Pandey.
This is an open-access article distributed under the terms of the Creative Commons Attribution License (CC BY). The use, distribution or reproduction in other forums is permitted, provided the original author(s) and the copyright owner(s) are credited and that the original publication in this journal is cited, in accordance with accepted academic practice. No use, distribution or reproduction is permitted which does not comply with these terms.
*Correspondence: Ratnesh K. Pandey, pandeyratneshk@gmail.com; Santosh Kumar, santosh.118365@stu.upes.ac.in
Disclaimer
All claims expressed in this article are solely those of the authors and do not necessarily represent those of their affiliated organizations, or those of the publisher, the editors and the reviewers. Any product that may be evaluated in this article or claim that may be made by its manufacturer is not guaranteed or endorsed by the publisher.