Abstract
FGH95–SiC composites containing 2.5–10 vol% SiC were fabricated by high-energy ball milling followed by spark plasma sintering (SPS). The effects of SiC content on the microstructure, crystallographic characteristics, hardness, and tribological behavior were systematically investigated. X-ray diffraction analysis confirmed the retention of the γ/γ′ matrix phases and SiC without detectable reaction products after SPS. The calculated γ/γ′ lattice misfit continuously decreased from 0.745% for monolithic FGH95% to 0.567% for the composite containing 10 vol% SiC, although a slight non-monotonic variation of the individual γ and γ′ lattice parameters was observed at the highest SiC content. Etched SEM observations and statistical grain-size analysis revealed only a slight decrease in average grain size from 1.15 ± 1.2 μm for FGH95 to 1.01 ± 1.0 μm for the 10 vol% SiC composite, with substantial overlap among the grain-size distributions. All specimens exhibited relative densities above 98%, indicating near-full densification, while the Vickers hardness increased from approximately 470–575 HV with increasing SiC content. Under sliding wear conditions, the wear rate decreased from approximately 5.2 × 10−4 to 2.9 × 10−4 mm3 N−1 m-1, corresponding to an improvement of approximately 45% at 10 vol% SiC. The worn-surface morphology revealed a transition from severe abrasive–delamination wear in monolithic FGH95 to predominantly mild abrasive wear in the SiC-reinforced composites. The enhanced wear resistance is primarily associated with the increased hardness and load-bearing capability of the uniformly dispersed SiC particles, together with the high densification and improved γ/γ′ crystallographic compatibility.
1 Introduction
Nickel-based superalloys are among the most important high-temperature structural materials owing to their exceptional mechanical strength, oxidation resistance, and creep resistance at elevated temperatures (; ; ). These outstanding properties make them indispensable for critical components in aerospace engines, gas turbines, and nuclear power systems, where materials are required to operate under severe mechanical and thermal loading conditions (; ). Their superior performance originates from the precipitation-strengthened γ/γ′ microstructure, in which coherent γ′ precipitates (Ni3(Al,Ti)) effectively impede dislocation motion and provide excellent high-temperature strength (; ). Among various powder metallurgy (PM) nickel-based superalloys, FGH95 has attracted considerable attention because of its high volume fraction of γ′ precipitates (approximately 45%–50%), excellent fatigue resistance, high tensile strength, and superior creep properties below 650 °C (; ; ; ). Compared with conventionally cast and wrought superalloys, PM-FGH95 exhibits a more homogeneous microstructure, finer grains, and reduced segregation, resulting in enhanced reliability for turbine disks and other rotating components subjected to cyclic loading. Nevertheless, with the continuous increase in service temperature and mechanical demands in next-generation aero-engines, conventional FGH95 alloys are approaching their performance limits (). Therefore, developing FGH95-based composites has emerged as an effective strategy for simultaneously improving strength, hardness, wear resistance, and thermal stability while maintaining acceptable ductility (; ; ; ). Ceramic particle reinforcement has been extensively investigated for strengthening metallic matrices because of the combined effects of load transfer, grain refinement, Orowan strengthening, and thermal expansion mismatch strengthening (; ; ). Among various ceramic reinforcements, silicon carbide (SiC) possesses several attractive characteristics, including high hardness, low density, excellent elastic modulus, superior thermal conductivity, low coefficient of thermal expansion, and remarkable chemical stability (; ; ; ). These properties enable SiC particles to effectively improve the stiffness, wear resistance, and high-temperature performance of metal matrix composites. In addition, the relatively low density of SiC makes it particularly attractive for lightweight aerospace structural materials, where high specific strength is required. Numerous studies have demonstrated that incorporating SiC particles into aluminum, magnesium, titanium, and copper matrices significantly enhances their mechanical and tribological properties (; ; ; ; ; ). The improvements are generally attributed to efficient load transfer from the metallic matrix to the stiff ceramic particles, grain refinement caused by particle pinning during sintering, and increased dislocation density generated by thermal expansion mismatch between the reinforcement and matrix. Furthermore, uniformly dispersed SiC particles can suppress grain growth during high-temperature processing, resulting in improved thermal stability and enhanced resistance to plastic deformation. However, these strengthening mechanisms strongly depend on the reinforcement content, particle distribution, interfacial bonding, and processing route. For nickel-based superalloys, incorporating ceramic reinforcements is considerably more challenging than in lightweight alloys. The high alloying content, complex γ/γ′ microstructure, and elevated processing temperatures may induce undesirable interfacial reactions between SiC and the nickel matrix, leading to the formation of brittle secondary phases or carbon-rich compounds. Excessive ceramic addition may also promote particle agglomeration, increase residual porosity, and deteriorate the continuity of the metallic matrix, thereby reducing ductility and fatigue resistance. Conversely, insufficient reinforcement content may not provide adequate strengthening to justify the additional processing complexity. Consequently, optimizing the SiC content is essential for achieving a desirable balance between microstructural stability and mechanical performance.
Powder metallurgy combined with spark plasma sintering (SPS) has become one of the most promising processing routes for fabricating nickel-based superalloy composites (; ). Compared with conventional hot pressing or hot isostatic pressing, SPS offers rapid heating rates, short sintering times, and localized Joule heating, which effectively suppress grain growth while promoting rapid densification (; ; ; ; ). These characteristics are particularly beneficial for retaining fine γ′ precipitates and minimizing undesirable interfacial reactions between ceramic reinforcements and the metallic matrix (). Moreover, the rapid sintering process facilitates a more homogeneous distribution of reinforcing particles and enables the fabrication of nearly fully dense composites with improved mechanical properties. Previous studies have demonstrated the effectiveness of various reinforcements for improving the mechanical performance of FGH95 and other Ni-based superalloys. For example, graphene nanosheet-reinforced FGH95 composites fabricated by powder metallurgy exhibited improved tensile properties at both room and elevated temperatures, demonstrating the potential of nanoscale reinforcement for strengthening the FGH95 matrix. However, the strengthening and failure behavior were strongly dependent on the reinforcement/matrix interface and temperature (). In related Ni-based superalloy systems, SiC has also been employed as a ceramic reinforcement. SiC-containing Inconel 625 composite coatings fabricated by laser cladding exhibited increased hardness and substantially improved wear resistance, which was associated with the formation of hard carbide phases and microstructural modification induced by SiC (). Recent work on SiC-modified GH3536 Ni-based superalloys further demonstrated that SiC can influence grain refinement, carbide formation, crystallographic texture, and mechanical properties (). Despite these advances, systematic studies of bulk SiC-reinforced FGH95 composites remain scarce. Most previous investigations have focused either on carbon-based reinforcements in FGH95 or on SiC-reinforced coatings and additively manufactured Ni-based alloys. In particular, the influence of SiC content on the densification, γ/γ′ crystallographic characteristics, hardness, and tribological behavior of bulk FGH95 composites fabricated by powder metallurgy and SPS has not been comprehensively established. Moreover, the relationship between SiC-induced changes in γ/γ′ lattice misfit and the resulting wear behavior remains insufficiently understood. Addressing this gap is important because FGH95 possesses a complex precipitation-strengthened γ/γ′ microstructure, and the interaction between ceramic reinforcement and this microstructure may differ substantially from that observed in conventional Ni-based matrices or surface coatings.
Accordingly, the present work systematically investigates FGH95–SiC bulk composites containing 2.5, 5, 7.5, and 10 vol% SiC fabricated by high-energy ball milling followed by SPS. The effects of SiC content on phase stability, SiC distribution, densification, γ/γ′ lattice parameters and lattice misfit, hardness, friction, and wear resistance are systematically evaluated. Particular emphasis is placed on establishing a processing, microstructure, property relationship and clarifying how SiC reinforcement modifies the deformation and wear mechanisms of the FGH95 matrix. The present study provides valuable insights into the design of high-performance FGH95-based composites for advanced aerospace and high-temperature structural applications.
2 Materials and methods
2.1 Materials
Commercial FGH95 nickel-based superalloy powder (Shanghai Knowhow Powder-Tech Co., Ltd., China) was employed as the matrix material. As shown in Figure 1a, the powder particles exhibited a nearly spherical morphology with an average particle size of approximately 30 μm. The detailed chemical composition of the FGH95 powder is listed in Table 1. Commercial SiC powder with an average particle size of approximately 16 μm (Figure 1b), supplied by Beckman Coulter Co., Ltd., was used as the reinforcement phase.
FIGURE 1
TABLE 1
| Elements | Cr | Co | Mo | W | Nb | Al | Ti | Ni |
|---|---|---|---|---|---|---|---|---|
| Content (wt%) | 13 | 8 | 3.3 | 3.5 | 3.7 | 3.3 | 2.5 | Balance |
Nominal chemical composition of the FGH95 superalloy powder (wt%); Ni is the balance element, including any minor/trace elements not individually listed.
2.2 Fabrication of FGH95/SiC composites
The fabrication process of SiC-reinforced FGH95 nickel-based superalloy composites is schematically illustrated in Figure 2a. Initially, FGH95 powder was blended with different SiC contents (2.5, 5.0, 7.5, and 10 vol%) using a high-energy planetary ball mill (PULVERISETTE 7, Fritsch, Germany). The ball milling process was carried out at a rotational speed of 300 rpm for 3 h with a ball-to-powder weight ratio of 4:1 to ensure homogeneous dispersion of the reinforcement particles. The mixed powders were subsequently consolidated by spark plasma sintering (SPS) using a Labox 350 system (Sinterland Inc., Japan). Prior to sintering, the powder mixtures were loaded into a graphite die and placed in a vacuum chamber to minimize oxidation during high-temperature processing. The SPS thermal profile, illustrated in Figure 2b, consisted of rapid heating to the target temperature, followed by an isothermal holding stage and controlled cooling. All specimens were sintered at 1,000 °C for 10 min under an applied pressure of 50 MPa. After SPS, fully consolidated bulk FGH95/SiC composite specimens were obtained for subsequent microstructural and property characterization.
FIGURE 2
2.3 Characterization
The microstructure, morphology, and surface characteristics of the sintered specimens were examined using a field-emission scanning electron microscope (FE-SEM, Hitachi S-4800, Japan). The elemental composition and elemental distribution were analyzed by energy-dispersive X-ray spectroscopy (EDS) equipped on a FE-SEM Hitachi S-4800 (Hitachi, Japan). To reveal the grain structure for grain-size analysis, the sintered composite specimens were first ground and polished using standard metallographic procedures. The polished surfaces were subsequently etched using an etchant consisting of 5 g CuCl2, 100 mL HCl, and 100 mL ethanol for 10 s. The etched surfaces were examined by SEM, and the grain-size distributions were obtained from the resulting micrographs using an ImageJ software. Phase identification and the formation of secondary phases were investigated by X-ray diffraction (XRD) using a Bruker D8 Advance diffractometer (Bruker, Germany). The XRD patterns were analyzed to identify the γ matrix, γ′ precipitates, and other secondary phases, as well as to evaluate phase evolution during the sintering process. The bulk density of the specimens was measured using the Archimedes method with an AND GR-202 density balance (A&D Co., Japan). The relative density was calculated as the ratio of the measured density to the theoretical density of the corresponding composite. The mechanical properties were evaluated by Vickers microhardness measurements using an AVK-CO microhardness tester (Mitutoyo, Japan). Hardness measurements were performed at multiple locations on each specimen to ensure statistical reliability. The tribological behavior was evaluated using a TRB3 tribometer (Anton Paar, Switzerland) under normal loads of 1 N and 5 N at a constant sliding speed of 5 cm s-1. The coefficient of friction (COF) was continuously recorded as a function of sliding distance under both normal loads. The wear rate was determined from the material volume loss after the wear test conducted under a normal load of 5 N. The morphology of the wear tracks was further examined using a Keyence VHX-X1 digital optical microscope (Keyence, Japan). To ensure the reliability and reproducibility of the experimental results, all reported data represent the average values obtained from at least five independent measurements for each specimen.
3 Results
3.1 Microstructure
The morphology of the ball-milled FGH95–SiC composite powders was characterized by SEM, and the corresponding EDS spectra are presented in Figure 3. As shown in Figure 3a, the FGH95 powder particles retained their nearly spherical to irregular morphology after high-energy ball milling, although noticeable plastic deformation and surface roughening were observed as a result of repeated collisions between the milling balls and powder particles. No severe cold welding or excessive agglomeration was observed, indicating that the selected milling parameters effectively promoted powder mixing while maintaining the integrity of the powder particles. The EDS spectrum collected from the overall powder mixture (Figure 3b) confirms the presence of the principal alloying elements of the FGH95 superalloy, including Ni, Cr, Co, Al, Ti, Mo, and W. Nickel is the dominant constituent, accounting for approximately 52.2 wt%, which agrees well with the nominal composition of the alloy. In addition, characteristic Si and C peaks were clearly detected, confirming the successful incorporation of SiC reinforcement into the FGH95 powder during the milling process. The absence of a significant oxygen peak suggests that oxidation during ball milling was effectively suppressed. A higher-magnification SEM image (Figure 3c) further reveals that the SiC particles were mechanically embedded and uniformly distributed on the surface of the FGH95 particles. The intimate contact between the ceramic particles and the metallic matrix indicates that repeated impact and shear forces during ball milling promoted mechanical anchoring of SiC onto the plastically deformed FGH95 powder surfaces. No obvious SiC agglomeration was observed within the examined region, suggesting that the milling process provided efficient dispersion of the reinforcement phase. Such a homogeneous distribution is expected to facilitate interfacial bonding during the subsequent spark plasma sintering process and minimize local stress concentrations in the consolidated composites. To verify the identity of the reinforcement phase, point EDS analysis was performed on the particle indicated in Figure 3c. As shown in Figure 3d, the EDS spectrum obtained from the selected particle shows characteristic signals of Si and C, with no detectable Ni, Cr, Co, or other major alloying elements. These results, together with the morphology, support the identification of the selected particle as SiC. The quantitative EDS values should be regarded as semi-quantitative because of the inherent limitations associated with the analysis of light elements, particularly carbon. Furthermore, no detectable Ni, Cr, or Co signals were observed in the analyzed region, indicating that the SiC particles retained their chemical stability during ball milling without undergoing any noticeable interfacial reaction with the FGH95 matrix. Therefore, the SEM and EDS results demonstrate that high-energy ball milling effectively dispersed the SiC reinforcement onto the surface of the FGH95 powder while preserving the chemical stability of both constituents. The intimate interfacial contact established during powder processing is expected to enhance diffusion bonding during spark plasma sintering, thereby improving densification and contributing to the enhanced mechanical and tribological properties of the FGH95/SiC composites.
FIGURE 3
The microstructure of the SPS-sintered FGH95–SiC composite and the corresponding point EDS analysis are presented in Figure 4. As shown in Figure 4a, the composite exhibits a dense microstructure with only a few isolated micropores, indicating that spark plasma sintering effectively consolidated the ball-milled powders. No obvious microcracks or interfacial debonding are observed around the reinforcement particles, suggesting the formation of a well-bonded interface between the SiC particles and the FGH95 matrix. The dark-contrast particles embedded in the metallic matrix are identified as SiC reinforcements. These particles are uniformly distributed throughout the matrix and remain well dispersed after the SPS process without severe agglomeration. Compared with the powder morphology before sintering, the reinforcement particles preserve their original morphology and are tightly anchored within the FGH95 matrix, indicating that the rapid heating and short holding time during SPS effectively suppressed particle coarsening while maintaining the homogeneous distribution achieved during ball milling. The point EDS spectrum collected from Position A (Figure 4b) reveals the presence of only Si and C, with weight fractions of 42.19 wt% and 57.81 wt%, respectively, confirming that the selected particle is SiC. No detectable Ni, Cr, Co, or other alloying elements are observed at this location, indicating that the reinforcement particles largely retained their chemical composition during the SPS process. Furthermore, no oxygen peak is detected, suggesting that oxidation of the SiC particles during sintering was negligible under the vacuum SPS environment. The absence of obvious reaction layers surrounding the SiC particles in the SEM image, together with the EDS results, suggests that no detectable interfacial reaction occurred between the FGH95 matrix and the SiC reinforcement under the selected SPS conditions (1,000 °C, 10 min, and 50 MPa). The excellent interfacial integrity is expected to facilitate efficient load transfer from the ductile matrix to the ceramic reinforcement while minimizing interfacial stress concentrations during mechanical loading.
FIGURE 4
To further characterize the microstructural evolution, the SPS-sintered specimens were metallographically etched and examined by SEM. The corresponding grain-size distributions are presented in Figure 5. More than 100 grains were analyzed for each composition. The average grain size decreases slightly from 1.15 ± 1.2 μm for monolithic FGH95 to 1.12 ± 1.1, 1.06 ± 1.1, 1.03 ± 1.0, and 1.01 ± 1.0 μm for the composites containing 2.5, 5, 7.5, and 10 vol% SiC, respectively. This corresponds to an overall reduction of approximately 12% at 10 vol% SiC. Although the results suggest a slight grain-refinement tendency with increasing SiC content, the grain-size distributions show substantial overlap and relatively large statistical variations. The porosity was not quantitatively determined from the etched SEM micrographs because all samples exhibited relative densities above 98%, indicating near-full densification. Therefore, the relative-density measurements were used to evaluate the densification behavior of the composites. The absence of a clear grain-size dependence on SiC content also suggests that the continuous increase in hardness should not be attributed primarily to grain refinement, but rather to the combined effects of SiC reinforcement, load transfer, dispersion strengthening, and dislocation obstruction.
FIGURE 5
3.2 Phase analysis
The XRD patterns of the ball-milled FGH95 powders reinforced with different SiC contents (2.5, 5, 7.5, and 10 vol%) are presented in Figure 6. The diffraction patterns of all samples are dominated by three characteristic peaks located at approximately 43.8°, 50.9°, and 74.8°, corresponding to the (111), (200), and (220) crystallographic planes of the γ/γ′ phases with a face-centered cubic (FCC) crystal structure. The persistence of these diffraction peaks indicates that the crystal structure of the FGH95 matrix remains stable after high-energy ball milling, irrespective of the SiC content. With the addition of SiC, a weak diffraction peak corresponding to the (102) plane of hexagonal SiC (PDF#29-1,131) appears at approximately 35.6°. The intensity of this peak gradually increases with increasing SiC content from 2.5 vol% to 10 vol%, confirming the successful incorporation of the ceramic reinforcement into the powder mixture. Nevertheless, the SiC peak remains relatively weak compared with those of the FGH95 matrix because of the relatively low reinforcement fraction and the significantly higher X-ray scattering intensity of the Ni-rich alloy matrix. No additional diffraction peaks associated with undesirable reaction products, such as nickel silicides or carbide phases, are detected in any of the composite powders. This observation indicates that no detectable chemical reaction occurred between the FGH95 matrix and SiC during the high-energy ball milling process. Therefore, SiC remained chemically stable and retained its original crystal structure after powder processing. Furthermore, the diffraction peaks of the FGH95 matrix exhibit slight broadening after ball milling, which can be attributed to grain refinement and the introduction of lattice defects caused by severe plastic deformation during repeated impact and shear events. The absence of noticeable peak shifts with increasing SiC content suggests that the reinforcement particles were primarily mechanically mixed with the alloy powder rather than dissolved into the γ matrix. Consequently, the lattice parameter of the FGH95 matrix remained essentially unchanged. The preservation of the γ/γ′ phases together with the absence of reaction products demonstrates that high-energy ball milling provides an effective route for uniformly dispersing SiC particles while maintaining the phase stability of the FGH95 superalloy. Such a stable powder structure is expected to promote subsequent densification during spark plasma sintering and preserve the intrinsic strengthening effect of the SiC reinforcement in the consolidated composites.
FIGURE 6
The XRD patterns of the SPS-sintered FGH95 and FGH95–SiC composites containing different SiC contents (2.5, 5, 7.5, and 10 vol%) are presented in Figure 7. The diffraction patterns of all specimens are dominated by three intense peaks located at approximately 43.6°, 51.0°, and 74.7°, corresponding to the (111), (200), and (220) planes of the γ/γ′ phases with a face-centered cubic (FCC) crystal structure. The retention of these characteristic diffraction peaks indicates that the FGH95 matrix maintains its original crystal structure after spark plasma sintering, demonstrating the excellent phase stability of the nickel-based superalloy under the selected SPS conditions. Compared with the monolithic FGH95 alloy, the composites exhibit several additional diffraction peaks located at approximately 35.6°, 40.9°, 46.0°, 59.8°, and 71.2°, which are indexed to the (102), (104), (107), (110), and (116) crystallographic planes of hexagonal SiC (PDF#29-1,131), respectively. The intensity of these SiC diffraction peaks gradually increases with increasing SiC content, confirming the successful retention of the ceramic reinforcement during the SPS process. The progressive increase in peak intensity is consistent with the increasing volume fraction of SiC incorporated into the FGH95 matrix. No additional diffraction peaks associated with undesirable reaction products, such as nickel silicides (Ni2Si or Ni3Si), titanium carbide (TiC), chromium carbides, or other secondary phases, are observed within the detection limit of XRD. This result suggests that the rapid heating rate and short holding time employed during SPS effectively suppressed extensive interfacial reactions between the SiC particles and the FGH95 matrix. Consequently, the SiC reinforcement remained chemically stable throughout the consolidation process. Furthermore, no pronounced shift of the γ/γ′ diffraction peaks is readily discernible from the overall XRD patterns in Figure 6 by direct visual comparison. However, because the (200) reflection consists of overlapping γ and γ′ contributions, subtle changes in the individual peak positions cannot be reliably resolved from the raw patterns alone. Therefore, the overlapped (200) reflection will be further deconvoluted to quantitatively determine the peak positions and lattice parameters of the γ and γ′ phases. Instead, the strengthening effect is primarily attributed to the physical incorporation of thermally stable SiC particles rather than solid-solution strengthening. The relatively sharp diffraction peaks of the γ/γ′ matrix also indicate that the crystallinity of the alloy was preserved after SPS, while the absence of significant peak broadening suggests that recovery and stress relaxation occurred during the sintering process, reducing the lattice strain introduced during high-energy ball milling. The preservation of both the γ/γ′ matrix and the SiC reinforcement demonstrates that spark plasma sintering provides an effective consolidation route for fabricating FGH95–SiC composites without inducing significant phase decomposition or interfacial reactions. Such phase stability is beneficial for maintaining the intrinsic high-temperature strength of the FGH95 superalloy while exploiting the high hardness and excellent wear resistance of the SiC reinforcement, thereby contributing to the improved mechanical and tribological performance of the composites.
FIGURE 7
To further clarify the influence of SiC reinforcement on the crystallographic characteristics of the FGH95 superalloy, the overlapped (200) diffraction peak was deconvoluted into the γ matrix and γ′ precipitate reflections using the Peak Fitting Module in Origin software, as shown in Figure 8. Using the peak positions labeled in Figure 8, the lattice parameters of the γ and γ′ phases were calculated according to Bragg’s law:
FIGURE 8
where Å (Cu Kα radiation). For the FCC crystal structure, the lattice parameter was determined from the (200) reflection using:
The lattice misfit between the γ and γ′ phases were calculated using:
The calculated lattice parameters together with the γ/γ′ lattice misfit are summarized in Table 2.
TABLE 2
| Sample | 2θγ (°) | 2θγ′ (°) | αγ (Å) | αγ′ (Å) | Lattice misfit (%) |
|---|---|---|---|---|---|
| FGH95 | 50.770 | 50.367 | 3.5937 | 3.6205 | 0.745 |
| FGH95–2.5 vol% SiC | 50.909 | 50.528 | 3.5845 | 3.6097 | 0.702 |
| FGH95–5 vol% SiC | 51.021 | 50.667 | 3.5772 | 3.6005 | 0.650 |
| FGH95–7.5 vol% SiC | 51.241 | 50.927 | 3.5628 | 3.5833 | 0.573 |
| FGH95–10 vol% SiC | 51.177 | 50.867 | 3.5670 | 3.5873 | 0.567 |
The calculated lattice parameters together with the γ/γ′ lattice misfit of the prepared composites.
The lattice parameters of both the γ and γ′ phases generally decrease with increasing SiC content up to 7.5 vol% SiC. At 10 vol% SiC, however, both phases exhibit a slight increase in lattice parameter, with αγ increasing from 3.5628 to 3.5670 Å and αγ′ increasing from 3.5833 to 3.5873 Å. The simultaneous variation of both phases suggests a modification of the overall lattice strain state rather than an isolated change in the γ phase. This behavior may be associated with changes in residual strain and defect structure induced by the increased SiC fraction during SPS and subsequent cooling, although the present XRD analysis cannot distinguish these contributions quantitatively. Importantly, the γ/γ′ lattice-parameter difference changes only slightly from 0.0205 Å to 0.0203 Å, and the calculated lattice misfit continues to decrease from 0.573% to 0.567%. Thus, the slight expansion of both phases at 10 vol% SiC does not represent a reversal of the γ/γ′ lattice-misfit trend. Direct verification of the underlying defect and strain evolution would require additional characterization, such as TEM-based dislocation-density analysis or local strain mapping. In addition, the deconvoluted (200) peaks provide clear evidence of a systematic peak shift with increasing SiC content. From monolithic FGH95 to the 7.5 vol% SiC composite, the γ peak shifts from 50.770° to 51.241°, while the γ′ peak shifts from 50.367° to 50.927°. According to Bragg’s law, the shift toward higher 2θ corresponds to a reduction in the interplanar spacing and, consequently, a decrease in the calculated lattice parameters. This trend is consistent with the progressive reduction in the γ/γ′ lattice misfit from 0.745% to 0.573%. For the 10 vol% SiC composite, both peaks exhibit a slight reverse shift toward lower 2θ, with the γ peak moving from 51.241° to 51.177° and the γ′ peak from 50.927° to 50.867°. Consequently, the lattice parameters increase slightly and the γ/γ′ lattice misfit remains nearly unchanged at 0.567%. This result indicates that the effect of further increasing the SiC content beyond 7.5 vol% on the γ/γ′ crystallographic relationship becomes relatively limited. This behavior is mainly attributed to two factors. First, the increasing amount of SiC reduces the effective volume fraction of the metallic γ matrix contributing to X-ray diffraction. Second, the thermal constraint imposed by the ceramic particles modifies the local strain state around the γ′ precipitates, leading to improved separation of the overlapping γ/γ′ peaks after deconvolution. The broader and relatively lower intensity of the γ peak observed in the composites containing 7.5 vol% and 10 vol% SiC also suggests an increase in microstrain and local lattice distortion caused by the higher fraction of rigid ceramic particles. The deconvoluted (200) reflection shows that the γ and γ′ peak positions systematically change with increasing SiC content. As summarized in Table 2, the separation between the γ and γ′ peaks decrease from 0.403° for monolithic FGH95 to 0.381°, 0.354°, 0.314°, and 0.310° for the composites containing 2.5, 5, 7.5, and 10 vol% SiC, respectively. This gradual reduction in peak separation is consistent with the calculated decrease in the γ/γ′ lattice misfit. It should be noted that the reduced peak separation does not necessarily indicate improved visual resolution of the two peaks; rather, it reflects the convergence of the γ and γ′ lattice parameters. The reduced peak separation reflects the convergence of the γ and γ′ lattice parameters and is consistent with the decrease in their calculated lattice misfit. The reduction in γ/γ′ lattice misfit from the monolithic alloy to the SiC-reinforced composites further supports this interpretation and suggests enhanced crystallographic compatibility between the two phases. As a result, the addition of SiC affects not only the lattice parameters but also the diffraction behavior of the γ and γ′ phases. The systematic shift of the (200) peaks toward higher diffraction angles confirms lattice contraction induced by residual compressive stresses, while the evolution of the peak intensities reflects changes in phase contribution and local lattice strain. These crystallographic modifications contribute to the enhanced precipitation strengthening and are expected to play an important role in the improved mechanical performance of the SPS-fabricated FGH95–SiC composites.
3.3 Density and hardness
The effects of SiC content on the relative density and Vickers hardness of the SPS-fabricated FGH95–SiC composites are presented in Figure 9. All specimens exhibit a relative density higher than 98%, indicating that spark plasma sintering effectively consolidated both the monolithic alloy and the SiC-reinforced composites. The relative density increases slightly from approximately 98.2% for monolithic FGH95 to nearly 99.0% for the composite containing 10 vol% SiC. The high densification is consistent with the rapid heating, applied pressure, and short holding time of the SPS process. Moreover, SEM observations reveal a relatively uniform distribution of SiC particles without obvious severe agglomeration, which is consistent with the high relative density observed for the SiC-reinforced composites. A more pronounced influence of SiC addition is observed in the hardness results (Figure 9b). The Vickers hardness increases continuously from approximately 470 HV for the monolithic FGH95 alloy to nearly 575 HV for the composite containing 10 vol% SiC, corresponding to an enhancement of about 22%. The progressive increase in hardness demonstrates that SiC is an effective reinforcing phase for improving the resistance to localized plastic deformation of the FGH95 matrix. The improvement in hardness originates from several concurrent strengthening mechanisms. First, the intrinsically high hardness and elastic modulus of SiC enable efficient load transfer from the ductile nickel matrix to the ceramic particles during indentation. Second, the uniformly dispersed SiC particles act as strong obstacles to dislocation motion, resulting in classical dispersion strengthening. The fine ceramic particles also reduce the effective dislocation mean free path, thereby increasing the critical stress required for plastic deformation. Furthermore, the thermal expansion mismatch between SiC and the FGH95 matrix generates geometrically necessary dislocations during cooling from the SPS temperature, producing additional dislocation strengthening. These effects operate simultaneously with the intrinsic γ/γ′ precipitation strengthening of the FGH95 alloy, leading to the continuous increase in hardness with increasing SiC content. The XRD analysis further supports the hardness evolution. As discussed previously, the addition of SiC up to 7.5 vol% decreases the γ/γ′ lattice misfit, indicating improved crystallographic coherency between the matrix and precipitates. Such coherent interfaces effectively impede dislocation motion, thereby enhancing precipitation strengthening. Although the lattice misfit increases slightly at 10 vol% SiC, the hardness continues to increase because the strengthening contribution from the larger volume fraction of hard SiC particles outweigh the slight reduction in crystallographic coherency. In addition, the SEM observations confirm that the SiC particles remain well bonded to the matrix after SPS, allowing efficient stress transfer across the particle–matrix interface.
FIGURE 9
3.4 Wear property
The tribological behavior of the SPS-fabricated FGH95–SiC composites with different SiC contents was evaluated under normal loads of 1 N and 5 N, and the corresponding friction coefficient curves and wear rates are presented in Figure 10. As shown in Figures 10a,b, all specimens exhibit a rapid increase in the coefficient of friction (COF) during the initial sliding stage, followed by a relatively stable steady-state region. The initial increase corresponds to the running-in stage, during which the asperities on the contact surfaces are progressively removed until a stable contact interface is established. After the initial running-in period, the COF generally enters a quasi-steady sliding regime, although noticeable local fluctuations are observed for some compositions. For example, the FGH95–7.5 vol% SiC composite exhibits a temporary increase in COF within approximately 125–175 m. Such fluctuations are likely associated with transient changes in the sliding contact, including local interactions between exposed SiC particles, the counterface, and wear debris. Nevertheless, the overall friction response after the running-in stage remains relatively stable compared with the initial sliding period. The addition of SiC has a pronounced influence on the friction behavior. Under a normal load of 1 N, the average COF initially increases from approximately 0.76 for the monolithic FGH95 alloy to about 0.91 for the composite containing 5 vol% SiC, followed by a significant decrease to approximately 0.72 for the composites reinforced with 7.5 and 10 vol% SiC (Figure 10c). A similar trend is observed under the higher normal load of 5 N, where the average COF reaches a maximum at 2.5–5 vol% SiC before decreasing continuously with further SiC addition, reaching the lowest value of approximately 0.66 for the 10 vol% SiC composite. The applied normal load has a noticeable influence on the friction behavior of the FGH95–SiC composites. Increasing the load from 1 to 5 N increases the mechanical contact between the specimen and counterface and promotes greater deformation of the asperities at the sliding interface. Consequently, the friction response becomes more strongly governed by the load-bearing capacity and hardness of the composite. At 1 N, the average COF increases from approximately 0.76 for monolithic FGH95 to approximately 0.91 for the 5 vol% SiC composite before decreasing to approximately 0.72 for the 7.5 and 10 vol% SiC composites. Under the higher load of 5 N, the COF reaches a maximum at relatively low SiC contents and subsequently decreases with increasing SiC content, reaching approximately 0.66 for the 10 vol% SiC composite. The lower friction coefficient at high SiC content under 5 N can be associated with the increased hardness and load-bearing capability of the composite, which suppress plastic deformation of the matrix and reduces severe ploughing at the sliding interface. These results indicate that the beneficial effect of SiC becomes more evident under the higher normal load, particularly at 7.5–10 vol% SiC. The increase in COF at relatively low SiC contents can be attributed to the increased surface roughness and the interaction between exposed hard SiC particles and the counterface, which enhances plowing and abrasive interactions during the initial stages of sliding. As the SiC content increases further, the higher hardness of the composites significantly suppresses plastic deformation of the matrix and improves the load-bearing capability of the sliding surface. Consequently, the real contact area between the composite and the counterface decreases, resulting in reduced adhesive interaction and a lower steady-state friction coefficient. The wear rate exhibits a continuous decrease with increasing SiC content, as illustrated in Figure 10d. The wear rate decreases from approximately 5.2 × 10−4 mm3N−1 m-1 for the monolithic FGH95 alloy to approximately 2.9 × 10−4 mm3N−1m-1 for the composite containing 10 vol% SiC, corresponding to an improvement of nearly 45% in wear resistance. This substantial reduction demonstrates that SiC reinforcement is highly effective in enhancing the tribological performance of the FGH95 superalloy.
FIGURE 10
The improved wear resistance is closely related to the microstructural evolution induced by SiC addition. The SEM observations confirmed that the SiC particles are uniformly distributed and well bonded to the FGH95 matrix after SPS, allowing efficient load transfer during sliding. In addition, the relative density of all composites exceeds 98%, indicating that the high densification achieved by SPS minimizes porosity, thereby reducing crack initiation sites and material removal during wear. More importantly, the continuous increase in hardness with increasing SiC content substantially improves the resistance of the matrix to plastic deformation and micro-cutting by abrasive asperities. The hard SiC particles also act as physical barriers that hinder subsurface dislocation motion and reduce the propagation of wear-induced deformation. The crystallographic analysis further supports the tribological behavior. As discussed previously, SiC addition up to 7.5 vol% reduces the γ/γ′ lattice misfit and enhances interfacial coherency between the γ matrix and γ′ precipitates, thereby increasing precipitation strengthening. Although the lattice misfit increases slightly at 10 vol% SiC, the greater volume fraction of hard SiC particles and the corresponding increase in hardness dominate the tribological response, resulting in the lowest wear rate among all investigated composites. It is noteworthy that the trends of friction coefficient and wear rate are not identical. While the wear rate decreases monotonically with increasing SiC content, the coefficient of friction exhibits a non-monotonic variation. This behavior indicates that friction and wear are governed by different mechanisms. The friction coefficient is mainly controlled by the nature of the sliding interface, including adhesion, surface roughness, and tribofilm formation, whereas the wear rate is primarily determined by the material’s resistance to plastic deformation and material removal. Therefore, a higher friction coefficient does not necessarily correspond to a higher wear rate. In conclusion, the incorporation of SiC significantly enhances the tribological performance of the FGH95 superalloy. The combination of high relative density, increased hardness, improved γ/γ′ interfacial coherency, and the load-bearing effect of uniformly dispersed SiC particles effectively suppresses plastic deformation and material removal during sliding. Consequently, the 10 vol% SiC composite exhibits the best wear resistance, whereas the 7.5–10 vol% SiC composites show the lowest steady-state friction coefficients under both loading conditions.
The three-dimensional optical micrographs and SEM images of the worn surfaces after the sliding wear tests are presented in Figures 11, 12, respectively. A clear evolution in the wear track morphology is observed with increasing SiC content. For the monolithic FGH95 alloy (Figures 11a, 12a), the wear track is relatively wide and deep, with a maximum wear depth of approximately 86 μm. The SEM image reveals numerous deep and continuous grooves parallel to the sliding direction, accompanied by severe plastic deformation and material removal. These features indicate that abrasive wear associated with plastic deformation is the dominant wear mechanism in the unreinforced alloy. After the incorporation of 2.5 vol% SiC (Figures 11b, 12b), the wear depth decreases significantly to approximately 26 μm, and the wear track becomes narrower and more uniform. Although parallel grooves are still visible, their depth and density are considerably reduced, indicating improved resistance to plastic deformation due to the presence of hard SiC particles. With further increasing the SiC content to 5 vol% (Figures 11c, 12c), the wear track remains relatively shallow (approximately 29 μm) and exhibits fewer severe grooves than the monolithic alloy. The worn surface becomes smoother, suggesting that the uniformly distributed SiC particles effectively hinder micro-cutting and suppress the propagation of plastic deformation during sliding. For the composites containing 7.5 and 10 vol% SiC (Figures 11d,e and 12 (d,e)), the worn surfaces become noticeably smoother, with only shallow grooves and limited material removal. The measured wear depths remain below 37 μm, which is substantially lower than that of the monolithic alloy. In particular, the 10 vol% SiC composite exhibits the narrowest and most uniform wear track, while the SEM image shows only fine scratches and the absence of severe ploughing or delamination. These observations indicate that the incorporation of a higher fraction of SiC significantly enhances the load-bearing capability of the composite and effectively suppresses severe wear damage. The morphological observations are consistent with the wear-rate measurements. As the SiC content increases, the reduction in wear depth and groove severity corresponds well with the continuous decrease in wear rate. The improved wear resistance can be attributed to the synergistic effects of increased hardness, excellent densification achieved by SPS, and the uniform distribution of SiC particles within the FGH95 matrix. The hard ceramic particles effectively restrict plastic deformation, reduce micro-cutting by the counterface, and inhibit crack initiation and propagation beneath the worn surface. Consequently, the dominant wear mechanism gradually changes from severe abrasive wear in the monolithic FGH95 alloy to mild abrasive wear in the SiC-reinforced composites. The observed tribological behavior can also be considered in relation to the intrinsic deformation and damage characteristics of SiC under abrasive contact. Previous studies have shown that SiC may undergo different material-removal regimes, ranging from brittle fracture to localized ductile deformation, depending on the contact and loading conditions (; ; ) further demonstrated that the friction and abrasive-wear behavior of SiC is closely coupled with local deformation and subsurface damage evolution. In the present FGH95–SiC composites, however, SiC acts as a dispersed reinforcing phase rather than as the bulk sliding material. Therefore, its principal contribution is associated with increasing surface hardness and load-bearing capability, thereby restricting severe plastic deformation and material removal of the FGH95 matrix. The tribological performance obtained in the present FGH95–SiC composites are broadly consistent with recent investigations of SiC-reinforced Ni-based materials. For example, SiC-reinforced Inconel 625 composite coatings have been reported to exhibit substantial increases in hardness and reductions in wear rate with increasing SiC content, with the maximum SiC-containing coating showing a wear-rate reduction of approximately 70% relative to the reference material (). Similarly, recent Ni–SiC composite coatings have demonstrated hardness values in the range of approximately 450–670 HV and improved wear resistance with increasing SiC incorporation (). In the present study, the hardness increased to 575 HV, while the wear rate reduced to 45% for the 10 vol% SiC composite. Although the magnitude of improvement is lower than that reported for some surface-engineered Ni–SiC coatings, the present results are significant because the composites are bulk FGH95 materials fabricated by high-energy ball milling and SPS rather than surface coatings. Moreover, the present work systematically investigates a relatively wide SiC-content range of 2.5–10 vol% and correlates SiC incorporation with γ/γ′ lattice misfit, hardness, friction, wear rate, and worn-surface evolution. These results demonstrate that SiC reinforcement provides an effective route for simultaneously modifying the mechanical and tribological response of bulk FGH95 superalloy.
FIGURE 11
FIGURE 12
To clarify the wear mechanism, high-magnification SEM images and the corresponding EDS spectra of the worn surfaces for the monolithic FGH95 alloy and the FGH95–10 vol% SiC composite is presented in Figure 13. The worn surface of the monolithic FGH95 alloy (Figures 13a1,a2) exhibits severe surface damage characterized by extensive delamination, large wear debris, deep cracks, and numerous craters formed by material removal. These features indicate that repeated sliding generated significant subsurface plastic deformation, leading to crack initiation and propagation parallel to the sliding surface. The propagation and coalescence of these cracks eventually resulted in the detachment of large fragments from the matrix, producing severe delamination wear. The abundant loose debris observed on the worn surface could further act as third-body abrasives, accelerating micro-cutting and aggravating surface damage. Therefore, the dominant wear mechanism of the monolithic alloy can be identified as abrasive wear accompanied by severe delamination wear. The EDS spectrum of the worn surface (Figure 13a3) reveals a remarkably high oxygen content (44.22 wt%) together with Ni, Cr, Co, and other alloying elements. A relatively high Fe content (30.11 wt%) was also detected, although Fe is not included in the nominal composition of the FGH95 alloy (Table 1). This Fe signal is most likely associated with material transfer from the Fe-containing counterpart during sliding, particularly given the severe abrasive and delamination wear observed on the FGH95 surface. Therefore, the Fe detected by EDS should not be considered an intrinsic constituent of the FGH95 matrix. The high oxygen concentration indicates that oxidation occurred during sliding due to frictional heating. However, the simultaneous presence of severe delamination, cracks, and fragmented debris suggests that the oxide layer formed on the FGH95 alloy was mechanically unstable and repeatedly fractured during sliding. Consequently, oxidative wear occurred simultaneously with abrasive and delamination wear rather than providing effective protection against material removal. In contrast, the worn surface of the FGH95–10 vol% SiC composite (Figures 13b1,b2) appears considerably smoother and more compact. Only a limited amount of fine wear debris is observed, while no obvious large cracks, craters, or delaminated regions are detected. The absence of severe plastic deformation indicates that the incorporation of SiC significantly enhances the load-bearing capability of the composite and effectively suppresses subsurface crack initiation during sliding. The uniformly distributed hard SiC particles increase the hardness of the composite and reduce the penetration depth of the counterface asperities, thereby minimizing micro-cutting and preventing extensive material removal. The EDS spectrum of the composite (Figure 13b3) further supports this interpretation. Compared with the monolithic alloy, the oxygen content decreases from 44.22 wt% to 33.34 wt%, indicating that oxidation during sliding is less severe. Meanwhile, the presence of carbon (10.68 wt%) and silicon confirms that SiC particles remain on or near the worn surface after the wear test, suggesting that the ceramic reinforcement actively participates in supporting the applied load and protecting the metallic matrix against direct contact with the counterface. The higher Ni content together with the lower Fe content compared with the monolithic alloy also indicates that material removal from the matrix is effectively reduced by the reinforcement. The improved wear resistance of the FGH95–10 vol% SiC composite can be attributed to the synergistic effects of several strengthening mechanisms. The high hardness of SiC restricts localized plastic deformation and serves as an effective barrier to dislocation motion. In addition, the excellent interfacial bonding achieved by spark plasma sintering allows efficient stress transfer between the matrix and the reinforcement, preventing premature particle pull-out during sliding. The higher relative density and reduced porosity further suppress crack initiation beneath the contact surface. Consequently, the dominant wear mechanism changes from severe abrasive–delamination wear in the monolithic alloy to mild abrasive wear with limited oxidative wear in the SiC-reinforced composite. These observations are in excellent agreement with the previously discussed hardness and wear-rate results. The continuous increase in hardness and the approximately 45% reduction in wear rate with increasing SiC content are directly associated with the suppression of crack formation, reduced delamination, and improved resistance to plastic deformation observed in the SEM images.
FIGURE 13
4 Conclusion
FGH95–SiC composites with different SiC contents were successfully fabricated by high-energy ball milling followed by spark plasma sintering. The results demonstrate that SiC incorporation provides an effective approach for tailoring the microstructural and tribological behavior of FGH95 while preserving the γ/γ′ matrix structure. The progressive reduction in γ/γ′ lattice misfit with increasing SiC content, together with the uniform dispersion of SiC particles and high densification, contributes to the enhanced hardness of the composites. These microstructural and mechanical changes are closely associated with the improved sliding-wear resistance, as reflected by the substantial reduction in wear rate and the transition from severe abrasive–delamination wear in monolithic FGH95 to predominantly mild abrasive wear in the SiC-reinforced composites. The results therefore establish a clear relationship between SiC reinforcement, microstructural stability, mechanical strengthening, and tribological performance. Among the investigated compositions, the 10 vol% SiC composite exhibited the most favorable combination of hardness and wear resistance, demonstrating the potential of SiC reinforcement for improving the wear performance of powder-metallurgy FGH95 superalloys.
Statements
Data availability statement
The raw data supporting the conclusions of this article will be made available by the authors, without undue reservation.
Author contributions
PV: Conceptualization, Formal Analysis, Investigation, Writing – original draft, Writing – review and editing. NA: Formal Analysis, Investigation, Methodology, Writing – original draft. TV: Data curation, Formal Analysis, Investigation, Writing – review and editing. NT: Formal Analysis, Investigation, Writing – review and editing. TT: Data curation, Formal Analysis, Investigation, Methodology, Writing – review and editing. DP: Conceptualization, Funding acquisition, Investigation, Project administration, Supervision, Writing – original draft, Writing – review and editing.
Funding
The author(s) declared that financial support was received for this work and/or its publication. This research is funded by Vietnam Academy os Science and Technology under project number NCPTVL.04/24-26.
Conflict of interest
The author(s) declared that this work was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.
Generative AI statement
The author(s) declared that generative AI was not used in the creation of this manuscript.
Any alternative text (alt text) provided alongside figures in this article has been generated by Frontiers with the support of artificial intelligence and reasonable efforts have been made to ensure accuracy, including review by the authors wherever possible. If you identify any issues, please contact us.
Publisher’s note
All claims expressed in this article are solely those of the authors and do not necessarily represent those of their affiliated organizations, or those of the publisher, the editors and the reviewers. Any product that may be evaluated in this article, or claim that may be made by its manufacturer, is not guaranteed or endorsed by the publisher.
References
1
ChenX.JiangN.ZhanY.LuoY.YeN.TangJ.et al (2024). Preparation and tribological performance of Ni-SiC composite coating on 304 stainless steel through brush plating. Surf. Coat. Technol.494, 131491. 10.1016/J.SURFCOAT.2024.131491
2
ChenJ.WangX.ZhouL.FuP.ChengY.ZhangH. (2025). Effect of refining temperature and refining time on purification and composition control of FGH95 powder metallurgy superalloy return material during vacuum induction melting. Metals15, 1140. 10.3390/MET15101140
3
Coyne-GrellA.BlaizotJ.RahimiS.ViolatosI.NouveauS.DumontC.et al (2022). Evolution of γ′ precipitation during the early stages of industrial forging of a nickel-based superalloy. Metallurgical Mater. Trans. A54, 2022–2036. 10.1007/S11661-022-06878-W
4
DonniniR.VaroneA.PalombiA.SpillerS.FerroP.AngellaG. (2025). High energy density welding of Ni-Based superalloys: an overview. Metals15, 30. 10.3390/MET15010030
5
GaoY.ZouJ.WangX.WangX.YangJ.WangH. (2020). Microstructure and mechanical performance of graphene nanosheets reinforced nickel-based superalloy FGH95 composite. Nanomaterials10, 100. 10.3390/NANO10010100
6
GudivadaG.PandeyA. K. (2023). Recent developments in nickel-based superalloys for gas turbine applications: review. J. Alloys Compd.963, 171128. 10.1016/J.JALLCOM.2023.171128
7
HeW. Q.KeP.HuangJ. Y.LiuF.TanL. M.HuangL.et al (2025). Mechanical properties and microstructural evolution of nickel-based superalloys. Trans. Nonferrous Metals Soc. China35, 2304–2319. 10.1016/S1003-6326(25)66816-6
8
IbrahimI. A.MohamedF. A.LaverniaE. J. (1991). Particulate reinforced metal matrix composites - a review. J. Mater. Sci.26, 1137–1156. 10.1007/BF00544448
9
JiangS.ChenY.XuC.SunS.ShaoX. (2026). Low-angle grain boundaries in Ni-Based single-crystal superalloys: formation mechanisms, microstructural features, and mechanical properties. Adv. Eng. Mater.28, e202502963. 10.1002/adem.202502963
10
JinD.LiuZ. (2011). Effect of cutting speed on surface integrity and chip morphology in high-speed machining of PM nickel-based superalloy FGH95. Int. J. Adv. Manuf. Technol.60, 893–899. 10.1007/S00170-011-3679-6
11
LaiL.NiuB.BiY.LiY.YangZ. (2023). Advancements in SiC-Reinforced metal matrix composites for high-performance electronic packaging: a review of thermo-mechanical properties and future trends. Micromachines14, 1491. 10.3390/MI14081491
12
LattanziL.Mohammadpour KasehgariS.AweS. A. (2025). The influence of SiC particle reinforcement on the thermophysical properties of aluminium-based metal matrix composites. J. Therm. Analysis Calorim.150, 10855–10866. 10.1007/S10973-025-14475-3
13
LiC.WangK.ZakharovO.CuiH.WuM.ZhaoT.et al (2025). Damage evolution mechanism and low-damage grinding technology of silicon carbide ceramics. Int. J. Extreme Manuf.7, 022015. 10.1088/2631-7990/ADA218
14
LiangZ.DengP.XiaoY.YanZ.HuangJ.ChenC.et al (2026). SiC induced in-situ modification: microstructure and properties of fine-grained SiC/GH3536 Ni-superalloy composites fabricated by laser powder bed fusion. J. Alloys Compd.1054, 186362. 10.1016/J.JALLCOM.2026.186362
15
LiuY.LiC.WangZ.GengY.ZakharovO.WangY.et al (2026). Damage evolution and abrasive wear behaviors involved in ultrafast laser-assisted grinding of SiC ceramics. Tribol. Int.214, 111264. 10.1016/J.TRIBOINT.2025.111264
16
MaS.ZhouS.ZhangW.WangS.LiuM. (2022). A facile synthesis of Inconel718-GNSs composites with high strength via spark plasma sintering. J. Alloys Compd.922, 166270. 10.1016/J.JALLCOM.2022.166270
17
OgunbiyiO. F.JamiruT.SadikuE. R.AdesinaO. T.BenekeL.AdegbolaT. A. (2019). Spark plasma sintering of nickel and nickel based alloys: a review. Procedia Manuf.35, 1324–1329. 10.1016/J.PROMFG.2019.05.022
18
OgunbiyiO.SadikuR.AdesinaO.AdesinaO. S.SalifuS.FayomiJ. (2021). Microstructure and mechanical properties of spark plasma-sintered graphene-reinforced inconel 738 low carbon superalloy. Metallurgical Mater. Trans. A53, 299–313. 10.1007/S11661-021-06525-W
19
PengH.ShiY.GongS.GuoH.ChenB. (2018). Microstructure, mechanical properties and cracking behaviour in a γ′-precipitation strengthened nickel-base superalloy fabricated by electron beam melting. Mater. Des.159, 155–169. 10.1016/J.MATDES.2018.08.054
20
QinZ.LiQ.WangG.LiuF. (2023). Microstructural characterization and prior particle boundary (PPB) of PM nickel-based superalloys by spark plasma sintering (SPS). Materials16, 4664. 10.3390/MA16134664
21
RibeiroY. D.SoaresA. C.OliveiraM. P.de OliveiraB. F.PereiraA. C.MonteiroS. N. (2022). Development and characterization of spark plasma sintered novel Ni, Cu, WC containing Nb-Based alloys for high-temperature applications. J. Mater. Res. Technol.17, 789–801. 10.1016/J.JMRT.2022.01.030
22
SalehB.FathiR.ZhaoL. (2026). Additive manufacturing of nickel superalloys: a critical review of recent advances and future perspectives. Appl. Mater. Today48, 103051. 10.1016/J.APMT.2025.103051
23
ShahbazkhanA.SabetH.AbbasiM. (2022). Investigation of bonding strength and hot corrosion behavior of NiCoCrAlSi high entropy alloy applied on IN-738 superalloy by SPS method. J. Alloys Compd.911, 164997. 10.1016/J.JALLCOM.2022.164997
24
SharathB. N. (2024). The effect of tertiary ceramic particle reinforcement on the mechanical characteristics of hybrid composites based on Al7029. J. Mater. Eng. Perform.34, 8504–8513. 10.1007/S11665-024-10220-3
25
ShuD. L.TianS. G.TianN.XieJ.SuY. (2017). Thermodynamic analysis of carbide precipitation and effect of its configuration on creep properties of FGH95 powder nickel-based superalloy. Mater. Sci. Eng. A700, 152–161. 10.1016/J.MSEA.2017.05.108
26
TianS.LiJ.ZhouX.LiA.LiangF. (2011). Constituting and distribution features of phases in FGH95 nickel base superalloy. Rare Met. 201130, 457–461. 10.1007/S12598-011-0324-3
27
TornabeneF.KonopkaK. (2022). Particle-reinforced ceramic matrix composites—selected examples. J. Compos. Sci.6, 178. 10.3390/JCS6060178
28
Van TrinhP.LeeJ.MinhP. N.PhuongD. D.HongS. H. (2018). Effect of oxidation of SiC particles on mechanical properties and wear behavior of SiCp/Al6061 composites. J. Alloys Compd.769, 282–292. 10.1016/J.JALLCOM.2018.07.355
29
Van TrinhP.LeeJ.KangB.MinhP. N.PhuongD. D.HongS. H. (2022). Mechanical and wear properties of SiCp/CNT/Al6061 hybrid metal matrix composites. Diam. Relat. Mater.124, 108952. 10.1016/J.DIAMOND.2022.108952
30
Van TrinhP.Binh AnN.Van HauT.TuanD.Van TuN.Thi HuyenN.et al (2025). SiC coated, CNT nanowire reinforced copper composite: preparation, microstructure and properties. RSC Adv.15, 48795–48806. 10.1039/D5RA05976C
31
WangY.MonettaT. (2023). Systematic study of preparation technology, microstructure characteristics and mechanical behaviors for SiC particle-reinforced metal matrix composites. J. Mater. Res. Technol.25, 7470–7497. 10.1016/J.JMRT.2023.07.145
32
WangY.WangH.LiuX.VecchioK. S. (2017). Microstructure evolution in Ni and Ni-superalloy based metallic-intermetallic laminate (MIL) composites. Intermet. (Barking)87, 70–80. 10.1016/J.INTERMET.2017.04.009
33
WangH.WuM.MiaoX.JinX.CuiC. (2024). Microstructure and wear resistance of SiC strengthened laser cladded Inconel625-Nb4-SiCx composite coatings. Mater. Today Commun.40, 109498. 10.1016/J.MTCOMM.2024.109498
34
WangK.ChenH.WuY.ZakharovO.GengY.LiC. (2025). Brittle-to-ductile transition depth and ductile deformation mechanisms during grinding of 4H-SiC crystals. Tribol. Int.212, 110972. 10.1016/J.TRIBOINT.2025.110972
35
WuQ.SiY.WangG. S.WangL. (2016). Machinability of a silicon carbide particle-reinforced metal matrix composite. RSC Adv.6, 21765–21775. 10.1039/C6RA00340K
36
WuW.ZengT.HaoW.JiangS. (2022). Microstructure and mechanical properties of aluminum matrix composites reinforced with in-situ TiB2 particles. Front. Mater.9, 817376. 10.3389/fmats.2022.817376
37
XieJ.TianS. G.LiJ. J.ZhouX. M.SuY. (2013). Influence of γ/γ’ lattice misfit on creep behaviours of FGH95 Ni based superalloy. Mater. Sci. Technol. (United Kingdom)29, 1021–1026. 10.1179/1743284713Y.0000000231
38
ZengX.LiuH.YangS.YuC.ChenM.WangF. (2025). Microstructure and mechanical properties of in-situ nano TiC reinforced Ni-based alloy composites prepared by spark plasma sintering. J. Mater. Sci. Technol.206, 100–112. 10.1016/J.JMST.2024.04.004
Summary
Keywords
FGH95, hardness, Ni-based superalloy, silicon carbide, spark plasma sintering, wear resistance
Citation
Van Trinh P, An NB, Van Hau T, Trinh ND, Trung TB and Phuong DD (2026) Microstructural evolution and tribological performance of SiC-reinforced FGH95 superalloy composites fabricated by spark plasma sintering. Front. Mater. 13:1953344. doi: 10.3389/fmats.2026.1953344
Received
30 July 2026
Revised
04 October 2026
Accepted
12 October 2026
Published
29 October 2026
Volume
13 - 2026
Edited by
Kaushik Kumar, Birla Institute of Technology, India
Reviewed by
Chen Li, Harbin Institute of Technology, China
Mohammad Reza Loghman Estarki, Malek Ashtar University of Technology - Shahin Shahr Campus, Iran
Updates
Copyright
© 2026 Van Trinh, An, Van Hau, Trinh, Trung and Phuong.
This is an open-access article distributed under the terms of the Creative Commons Attribution License (CC BY). The use, distribution or reproduction in other forums is permitted, provided the original author(s) and the copyright owner(s) are credited and that the original publication in this journal is cited, in accordance with accepted academic practice. No use, distribution or reproduction is permitted which does not comply with these terms.
*Correspondence: Pham Van Trinh, trinhpv@ims.vast.vn; Doan Dinh Phuong, phuongdd@ims.vast.ac.vn
Disclaimer
All claims expressed in this article are solely those of the authors and do not necessarily represent those of their affiliated organizations, or those of the publisher, the editors and the reviewers. Any product that may be evaluated in this article or claim that may be made by its manufacturer is not guaranteed or endorsed by the publisher.