A comprehensive review on development of texture in automotive-grade medium manganese steel

  • 1. School of Mechanical Sciences, Odisha University of Technology and Research, Bhubaneswar, India

  • 2. Department of Mechanical Engineering, National Institute of Advanced Manufacturing Technology, Ranchi, India

Abstract

Medium manganese steels (MMnSs, 3–12 wt% Mn) are pivotal for third-generation automotive applications due to their strong strength-ductility synergy from complex phase transformations and texture evolution. This review discusses the latest findings in texture development across ferritic, austenitic, and duplex MMnSs, focusing on the influence of alloying elements, stacking fault energy (SFE), and austenite reversion during processing. Studies show that γ-fiber strengthening, cube orientation, and twinning-induced reorientation affect mechanical anisotropy and crashworthiness. Key elements like Mn, Ni, and C stabilize austenite and foster γ-fiber textures, while Al and Si decrease SFE to enhance twinning and ferritic cube components. Despite significant progress, challenges in predicting quantitative prediction of texture evolution under industrial processing conditions, the stability of reverted austenite during cyclic loading, and the integration of TRIP/TWIP mechanisms into predictive models persist. Research gaps include the need for advanced in-situ characterization, multiscale simulations linking chemistry to texture, and long-term corrosion-mechanical coupling studies. By identifying these challenges, this review provides a roadmap for alloy design and processing strategies aimed at optimizing the strength–ductility balance of MMnSs for next-generation automotive steels.

1 Introduction

1.1 Background

The automotive industry is actively working to enhance fuel efficiency and component performance while simultaneously reducing CO2 emissions and vehicle weight (Raabe et al., 2009; Ma et al., 2020; Suh and Kim, 2017; Li et al., 2018a; Yadav et al., 2023). A significant development in this effort is the use of advanced high-strength steels (AHSSs), which are recognized for their lightweight characteristics (Figure 1). AHSS has exceptional ductility, toughness, and fatigue resistance, making it suitable for various vital components of vehicles, including undercarriages, vehicle bodies, frames, bumpers, and doors (De Cooman et al., 2012). AHSS is categorized into three generations (Soleimani et al., 2020; Chen et al., 2017; Lee and Han, 2015; Hu et al., 2019; Zhang et al., 2018): (1) The first-generation AHSS includes low-Mn martensitic steels, transformation-induced plasticity (TRIP) steels, dual-phase (DP) steels, and complex-phase (CP) steels, which are designed to improve vehicle performance and safety (Zou et al., 2017; Li ZC. et al., 2017; Zhou et al., 2018). (2) The second generation introduces twinning-induced plasticity steels, nano-twinning-induced plasticity (TWIP) steels, and duplex and triplex steels, which address issues of lower ductility found in first-generation materials (Dalai et al., 2026). These are applied in structural components, barrier systems, and various safety features in vehicles (Sun et al., 2022; Mohapatra et al., 2026a). (3) Third-generation AHSS, which includes medium-manganese steel (MMnS) (Cai et al., 2016; Mishra et al., 2017; Dutta et al., 2019; Mohapatra et al., 2023a), quenching and partitioning (Q&P) steel (Zinsaz-borujerdi et al., 2018; Dai et al., 2018; Seo et al., 2016; Hu et al., 2023), and carbide-free bainite (CFB) steel (Bhadeshia, 2005; Soliman and Palkowski, 2014), has gained traction due to its ability to further lower CO2 emissions and enhance fuel efficiency. MMnSs are particularly notable for their superior strength-to-elongation ratios and are cost-effective alternatives to high-manganese TWIP steels. TWIP, TRIP, ferritic-bainitic (FB), and martensitic (MS) steels also significantly contribute to structural integrity and safety standards in automotive manufacturing.

FIGURE 1

1.2 Automotive-grade medium manganese steel (MMnS)

MMnS with 3–12 wt% Mn is proposed as a viable option for third-generation AHSS, aiming to achieve an optimal balance of strength and ductility while minimizing production costs and enhancing crash resistance (Lee and Han, 2015; Hu et al., 2017; Dalai et al., 2023; Mohapatra, 2023; Mohapatra et al., 2026b; Wang et al., 2019). The demand for lightweight Fe-Mn-Al-C MMnS has surged due to their favorable tensile properties and reduced density, which are advantageous for automotive applications (Mohapatra et al., 2022; Yu and Deng, 2025). The density regulation of these steels is influenced by aluminum (Al) content; although higher Al levels lower density, they also lead to the formation of non-metallic Al inclusions such as Al2O3 and Fe3Al intermetallic compounds, which can adversely affect the desired strength-ductility combination in these advanced materials. Consequently, maintaining a limited Al concentration in AHSS is crucial to prevent the development of brittle intermetallic precipitates. These steels can be classified into three categories: ferritic, austenitic, and duplex steels, which comprise both ferrite and austenite phases (Hui et al., 2017; Shao et al., 2017). The tensile properties of single-phase ferritic steel can be enhanced through the generation of the austenite phase during various heat treatments and the transformation of unstable austenite into martensite during tensile stress application, leveraging the TRIP effect (Zou et al., 2017; Luo et al., 2017; Pütz et al., 2021). The latest generation of AHSS utilizes TRIP to optimize the interplay between strength and ductility, significantly enhancing work hardening behavior and this key relationship. Furthermore, the introduction of alloying elements such as nickel (Ni) can improve the strength-ductility relationship via mechanisms of precipitation and solid solution strengthening. Studies have shown that integrating TRIP mechanisms with B2(NiAl) precipitation can result in exceptional tensile properties in nickel-enriched MMnS (Lee et al., 2013; Peng et al., 2018; Han et al., 2011; Kumar et al., 2023; Cheng et al., 2019; Cai et al., 2014).

Common processing techniques used in MMnS include intercritical annealing (IA), quenching and partitioning (Q&P), and quenching and tempering (Q&T) (Li et al., 2018a; Mohapatra et al., 2023b; Li et al., 2016). Different initial microstructures prior to IA can influence the morphology of RA. Austenite reversion and precipitation are influenced by hot and cold deformation prior to heat treatment. Nevertheless, the formation of sizable precipitates requires further annealing treatment. Through adequate element partitioning, IA can generate a suitable amount of austenite to facilitate stabilization. A novel method of moderate temperature modulation allows for the continuous reversion of austenite while also promoting nanoprecipitation. The mechanical performance of medium Mn steels is contingent upon the microstructure optimization of retained austenite (RA) and nano-sized particles. The design of a new steel with a suitable IA processing window, along with enhanced RA stability, is of utmost importance to achieve the optimal TRIP effect (Sahoo et al., 2021; Poojari et al., 2024; Han et al., 2017). The presence of RA stabilizes the TRIP and TWIP mechanisms, leading to enhanced strain hardening. The uniform precipitation of nano-sized particles is closely associated with segregation, while the morphology and mechanical stability of austenite can be regulated by element diffusion. Metastable austenite with varying micro-mechanical stability is the result of cold deformation prior to austenite reversion treatment, which is attributed to the non-uniform distribution of element content, grain size, and dislocation density. The interface migration rate of the kinematic growth mode is regulated by Mn diffusion across the austenite/ferrite phase boundaries. Mn segregation favorably to precipitates can significantly influence TRIP effects by reducing the concentration in solid solution and the stacking fault energy (SFE) of austenite (Li ZC. et al., 2017; Hui et al., 2017; Shao et al., 2017; Li et al., 2018b; Steineder et al., 2017).

1.3 Importance of texture in automotive applications

Texture plays a crucial role in automotive applications, particularly in the mechanical anisotropy, formability, and crashworthiness of advanced steels utilized in vehicle structures (Xie and Nakamachi, 2002; Raabe, 1997; Mohapatra et al., 2024a). Its importance can be dissected into several key aspects: Automotive body panels necessitate superior deep-drawing performance. A strong γ-fiber ({111}//ND) texture enhances the plastic strain ratio (r-value), which in turn minimizes thinning and heightens sheet formability. This leads to smoother stamping processes and reduces manufacturing defects. Texture is instrumental in dictating the distribution of slip systems and twinning mechanisms within the steel. An optimized combination of γ-fiber and cube textures enables the achievement of the TRIP and TWIP effects (Mandal, 2016). This balance is critical for developing lightweight yet crash-resistant automotive designs. The influence of texture extends to the strain hardening behavior and uniform elongation of the material. Steels with refined γ-fiber textures demonstrate higher strain hardening rates, allowing them to absorb more energy in the event of an impact, thus significantly enhancing passenger safety during crashes (Mohapatra et al., 2026b; Mohapatra et al., 2023c). Poorly controlled textures can lead to mechanical anisotropy, which results in uneven deformation in vehicle panels. By managing texture evolution effectively, manufacturers can ensure isotropy, reduce spring back and enhance dimensional accuracy in automotive components. Texture also affects the distribution of grain boundary characters, specifically CSL boundaries. Optimized texture variations increase the prevalence of these special boundaries, thereby improving resistance to intergranular corrosion and fatigue cracking—vital for the long-term durability of vehicles. The details of different texture components and their importance are presented in Table 1.

TABLE 1

Texture componentAutomotive impact
γ-fiber ({111}//ND)High plastic strain ratio, excellent deep drawability, improved ductility
Cube ({001} <100>)Balanced isotropy, reduced springback, dimensional accuracy
Goss ({110} <001>)Influences recrystallization, can reduce anisotropy if controlled
Brass ({110} <112>)Associated with deformation twinning, enhances strain hardening

Automotive relevance of key texture components in MMnSs, highlighting their influence on formability, anisotropy, and strain-hardening behavior.

1.4 Scope of this review

This paper provides a comprehensive synthesis of texture development in MMnS, structured as follows:

This review work comprehensively synthesizes texture development in automotive-grade-MMnSs. It systematically compares ferritic, austenitic, and duplex MMnSs classes, linking texture components to mechanisms (TRIP/TWIP) and mechanical implications. The manuscript highlights the influence of alloying elements (Mn, Ni, C, Al, and Si) on SFE and texture evolution. It connects microstructural observations to automotive applications, discussing anisotropy, establishing texture evolution as the central design parameter for optimizing strength-ductility balance in next-generation automotive steels.

2 Evolution of texture

Texture-induced anisotropy significantly influences the deep drawability and formability properties, YS, and elastic modulus of BCC steels (Xie and Nakamachi, 2002; Raabe, 1997; Mohapatra et al., 2024a). The properties are enhanced by the ND or γ-fibers present in the ferrite phase, whereas cleavage fractures are propagated by the (001) planes in BCC materials (Ghosh et al., 2014). Delamination behavior is adversely affected by the cube fiber texture, specifically the (001) 〈110〉 orientation (Ghosh et al., 2016). Thus, it is more advantageous to deduce from previous research that the formation of cube fibers should be limited to achieve superior tensile properties. The YS is reportedly enhanced when the transformation texture contains a greater proportion of fibers in the (113) 〈110〉 orientation, which is a substantial constituent of RD//〈110〉 fiber (Hutchinson et al., 2005). Like the BCC phase, the tensile properties are significantly influenced by the textural components of the FCC phase. Barbier et al. explained that superior tensile properties can be achieved by incorporating brass component texture intensities into high-manganese TWIP steel during deformation (Barbier et al., 2009). However, MMnS exhibits distinct characteristics. The following are some of the studies conducted on the evolution of texture and its correlation with the mechanical behavior of MMnS.

2.1 Rolling texture in FCC-austenite phase

The SFE of the material influences the evolution of textural components of the FCC-austenite phase (Suwas et al., 2014; Capek et al., 2018). Materials with lower SFE exhibit the formation of brass-type (110) < 1 2> and Goss-type (011) 〈100〉 components, while materials with higher SFE develop Cu-type (112) 〈111〉 components (Suwas et al., 2014). The α, τ, and β phases are the primary sources of fibers for the FCC-austenite phase. The primary texture fiber is composed of brass, Cu, and cube components, specifically the α-fiber (〈011〉//ND) (Raabe, 1997).The α-fiber of the FCC phase shifts from the Goss component (110) 〈001〉 to the brass component (110) <1 2> (Pradhan et al., 2024). The τ-fiber of the FCC phase, oriented along the 〈110〉 direction with respect to the transverse direction (TD), extends from the (001) 〈110〉 plane through the Cu position to the Goss components located at the (110) 〈001〉 plane Figure 2a (Raabe, 1997; Suwas et al., 2014; Capek et al., 2018). The β-fiber is an asymmetrical fiber that spans from the Cu location (112) 〈111〉 to the α-fiber at the brass position (110) <1 2> through the S orientation (123) 〈634〉 (Raabe, 1997; Suwas et al., 2014). Figure 2b illustrates the ideal orientations for FCC-austenite in Euler’s space at ϕ2 = 45°.

FIGURE 2

2.2 Rolling texture in BCC-ferrite phase

The BCC-ferrite phase of BCC metals is characterized by the development of textural elements, such as α, γ, η, and ε fibers, which are associated with a specific fiber orientation in Euler’s space (Xie and Nakamachi, 2002). The terms “RD” and “ND” fibers correspond to α- and γ-fibers, respectively. Figure 3 shows the optimal orientations for BCC-ferrite in Euler’s space, specifically at a ϕ2 angle of 45°. The RD fiber extends from (001) 〈110〉 to (111) 〈110〉 in the φ1 direction, whereas the ND fiber extends from (111) 〈110〉 to (111) 〈112〉 along the φ1 direction (Suwas et al., 2014).

FIGURE 3

3 Microstructural classes and texture mechanisms in medium manganese steels

3.1 Ferritic medium manganese steels (3–6 wt% Mn)

Ferritic MMnSs multi-phase microstructures exhibit distinct microstructural characteristics, primarily featuring an α ferrite matrix with dispersed retained or reverted γ austenite. The low Mn content stabilizes the ferrite phase, while small amounts of austenite are retained due to carbon partitioning during the intercritical annealing process. This ferritic matrix contributes to high yield strength and dimensional stability; however, it presents limited ductility unless aided by the TRIP effect attributable to austenite. Regarding texture development, ferritic MMnSs show pronounced cube ({001}//ND) and α fiber ({110}//RD) orientations (Jia et al., 2017). It was observed that cube texture becomes dominant post-intercritical annealing, with α fiber textures developing primarily during the rolling process. Although the minor γ austenite fraction introduces weak γ fiber ({111}//RD) orientations, its overall influence is substantially lower than that observed in duplex steels (Song et al., 2018). Mechanistically, dislocation slip serves as the primary mode of deformation due to moderate SFE. The TRIP effect enhances ductility as retained austenite transforms into martensite under stress. Additionally, the texture stability in ferritic MMnS is notably high, as ferrite demonstrates resistance to reorientation during deformation processes. In terms of applications, ferritic MMnSs are well-suited for scenarios demanding high yield strength and dimensional stability. However, their design makes them less favorable for deep drawability, primarily due to the limited strengthening provided by the γ fiber orientations. Ferritic MMnSs are dominated by an α-ferrite matrix with dispersed retained or reverted γ-austenite. The relatively low Mn content stabilizes ferrite, while small fractions of austenite are retained through carbon partitioning during intercritical annealing. The ferritic matrix provides high yield strength and dimensional stability, but ductility is limited unless austenite contributes via TRIP (Zhao et al., 2023).

3.2 Austenitic medium manganese steels (9–12 wt% Mn)

Austenitic-MMnSs are characterized by a predominant γ austenitic structure, stabilized thermodynamically by high Mn and Ni content, with carbon partitioning during annealing further enhancing this stability (Cai et al., 2016; Zhang et al., 2020). The SFE within these steels are at levels that effectively inhibit martensitic transformation while allowing for mechanical twinning, which plays a crucial role in the material’s mechanical behavior (Wang et al., 2023). These steels are noted for developing robust γ fiber textures, specifically aligned along the {111} direction relative to the rolling direction (RD). Researchers have established that mechanical twinning aids in the reorientation of grains toward {111} and {110} orientations, thereby strengthening the γ fiber and significantly contributing to enhanced ductility (Xu et al., 2025). Furthermore, EBSD studies have shown that TWIP is a dominant mechanism in the texture evolution of these materials. Key mechanistic insights include the TWIP effect, which refers to how mechanical twinning reinforces the γ fiber; the influence of high SFE owing to the presence of Mn, Ni, and carbon, promoting slip and twinning instead of martensitic transformation; and the dynamic evolution of texture, where the γ fiber becomes more pronounced with increasing strain, leading to improved formability. From a practical perspective, austenitic MMnSs are particularly suited for applications necessitating exceptional ductility and formability. However, their significant manganese content raises production costs, and their overall strength remains lower compared to duplex steels, suggesting a trade-off between ductility benefits and economic factors alongside strength considerations (Liu et al., 2018). Austenitic-MMnSs are fully or predominantly γ-austenitic. High Mn and Ni contents stabilize austenite thermodynamically, while carbon partitioning during annealing further enhances stability. These steels exhibit SFE in the range that suppresses martensitic transformation but permits mechanical twinning.

3.3 Duplex medium manganese steels (6–9 wt% Mn)

Duplex-MMnSs feature a dual-phase structure comprising balanced amounts of ferritic and austenitic phases. The process of intercritical annealing facilitates carbon partitioning into the austenite phase, resulting in fine reverted γ networks embedded within the ferrite matrix (Varanasi et al., 2022). This specific microstructure fosters both TRIP and Twinning-Induced Plasticity TWIP mechanisms to operate simultaneously, augmenting overall mechanical performance (Zhang et al., 2022). In terms of texture development, duplex MMnSs exhibit intricate textural characteristics. The ferritic phase develops orientations aligned with cube and α fibers, while the reverted austenite phase fortifies the γ fiber orientations. Additionally, twinning within the austenite introduces new components along the {111} and {110} directions. These synergistic textures in duplex steels contribute to a favorable balance of strength and ductility, positioning them as superior choices within the category of high-performance materials (Lee et al., 2018). Mechanistically, the TRIP effect leads to the transformation of austenite into martensite, which significantly boosts the material’s strength (Li et al., 2024). Conversely, the TWIP effect entails grain reorientation through twinning, enhancing ductility (Bai et al., 2021). Furthermore, the synergy between the textures of the ferrite and austenite phases offers isotropic properties alongside improved formability, crucial for numerous applications. The implications of these characteristics underscore the significance of duplex MMnSs in automotive applications. They achieve remarkable tensile strength due to the presence of ferrite and martensite while ensuring sufficient ductility via austenite and twinning phenomena. The complexity of texture evolution within duplex steels serves to provide the most advantageous mechanical properties, solidifying their role as a technologically relevant class of materials in modern engineering.

4 Role of alloying elements in texture development

4.1 Influence of manganese (Mn)

Mn promotes γ-fiber ({111}//RD) strengthening, enhancing ductility and formability. In duplex steels, Mn ensures sufficient austenite fraction to balance ferritic cube orientations. Mn plays crucial roles in the development of texture in medium-Mn steels, influencing various key aspects. It enhances the stability of γ-austenite by lowering the SFE, which delays martensitic transformation and facilitates TRIP and TWIP during deformation (Grajcar et al., 2018). The maintenance of γ-fiber texture is essential for achieving high ductility and toughness in these materials. The content of Mn significantly affects recrystallization and deformation textures; notably, steels with 6–10 wt% Mn exhibit distinct differences in deformation kinetics and texture development compared to those with lower Mn concentrations (Singh et al., 2023). Higher Mn levels disrupt the equilibrium between ferrite and austenite, leading to variations in orientation distribution and grain boundary character. Moreover, Mn promotes austenite reversion during intercritical annealing, influencing both the morphology and orientation of the reverted austenite, with the initial microstructure and Mn content playing a critical role in the kinetics of this reversion and the uniformity of the resulting texture (Zuo et al., 2026). At elevated concentrations, Mn enhances SFE, which encourages twinning, while at moderate concentrations, it balances TRIP and TWIP mechanisms, thereby refining the texture. Additionally, Mn alters the proportion of coincidence site lattice (CSL) boundaries, which contribute to improved mechanical performance and corrosion resistance. The document also highlights the synergistic interaction of Mn with aluminum and silicon, which refines bainitic/ferritic matrices and stabilizes retained austenite. However, excessive Mn may compromise corrosion resistance due to segregation issues (Mohapatra et al., 2026c). The study underscores the importance of predictive modeling that comprehensively incorporates Mn’s influence on TRIP and TWIP in texture evolution models. Optimizing Mn content is deemed necessary for achieving a balance among mechanical strength, ductility, and corrosion resistance (Mohapatra et al., 2023d). Furthermore, pilot trials are recommended to validate the role of Mn in texture retention during processes like continuous annealing and hot press forming. In summary, manganese is vital for enhancing the mechanical properties of MMnSs while requiring careful management to avoid potential downsides related to corrosion resistance. The effect of manganese alloying on texture evolution and mechanical response is presented in Table 2.

TABLE 2

Mn contentTexture effectMicrostructural impactMechanical consequence
Low (<5 wt%)Weak γ-fiber, faster recrystallizationLimited retained austeniteHigher ductility, lower strength
Medium (6–10 wt%)Strong γ-fiber + cube texturesStable retained austenite, balanced TRIP/TWIPOptimal strength–ductility balance
High (>12 wt%)Excess γ-fiber, delayed recrystallizationSegregation, risk of brittle phasesHigh strength, reduced toughness

Influence of manganese content on texture evolution, microstructural stability, and resulting strength–ductility balance in MMnSs.

4.2 Effect of nickel (Ni)

Ni plays a crucial role in the development of material texture, primarily through its effects on austenite stabilization, grain refinement, orientation control, and slip system activation (Cen et al., 2022). During intercritical annealing, Ni preferentially partitions into austenite, which increases its stability. This process enhances the fraction of RA, effectively delaying the martensitic transformation and fortifying the TRIP and TWIP mechanisms. The addition of Ni leads to finer grains in both ferrite and austenite. This refinement reduces texture heterogeneity and promotes the critical γ-fiber texture, oriented as 〈111〉//ND, which is essential for enhancing ductility and toughness (Xia et al., 2020). Steels containing Ni exhibit improved activation of slip systems in both FCC austenite and BCC ferrite phases (Kumar et al., 2025a). This augmentation enhances the strain hardening response, allowing for greater uniform deformation and delaying necking during mechanical stress. The behavior of Ni in partitioning contributes to austenite stability and suppresses premature transformations (Zhang et al., 2020). More stable RA enhances the TRIP effect, leading to improved elongation in the material. Additionally, Ni facilitates the formation of twin boundaries and increases γ-fiber intensity, linking microstructural characteristics with tensile properties. Even small additions of Ni (approximately 1 wt%) can yield performance benefits that surpass those of higher Mn steels in terms of the strength-ductility balance (Kumar et al., 2023). The significant role of Ni in promoting γ-fiber texture and twin boundaries is vital for tailoring the anisotropy of sheet steels (Kumar et al., 2025a). The properties imparted by Ni in comparison to high-Mn steels mitigate risks of banding and segregation, making Ni-containing steels more desirable for various applications such as welding and forming, thus highlighting its industrial relevance. Comparative impact of nickel content on texture development, microstructural refinement, and mechanical performance in MMnSs is shown in Table 3.

TABLE 3

Ni contentTexture effectMicrostructural impactMechanical consequence
0 wt%Weaker γ-fiber, less RA stabilityCoarser grains, heterogeneous textureLower ductility, unstable TRIP
∼1 wt%Strong γ-fiber, refined grainsStable RA, enhanced twin boundariesExcellent strength–ductility synergy
>2 wt%Excess stabilization, risk of cost issuesOver-refined grains, reduced TRIP efficiencyHigh ductility, but less economical

Effect of nickel content on texture evolution, microstructural refinement, and strength–ductility balance in MMnSs.

4.3 Role of carbon (C)

During intercritical annealing, carbon preferentially diffuses into austenite which stabilizes the retained austenite at room temperature (Li Y. et al., 2017). This process enriches austenite, promoting a γ-fiber texture ({111} that later transforms into advantageous orientations in ferrite post-deformation. A higher carbon content also delays the recrystallization of ferrite, allowing deformation textures to persist for extended periods (Aliabad et al., 2025). Carbon plays a critical role in the kinetics of cementite precipitation and dissolution when combined with manganese. Fine cementite particles help pin grain boundaries, which slows down recrystallization and sharpens the resulting texture (Lamari et al., 2026). During annealing, the controlled dissolution of cementite releases carbon back into the austenite, thereby enhancing the uniformity of the texture. In medium-Mn steels, carbon influences the driving force for the transformation of martensite back to austenite upon heating. This transformation is significant as it leads to the development of cube and Goss textures in reverted austenite, which subsequently impact mechanical anisotropy. While carbon in solid solution increases strength, it can also diminish toughness if austenite levels are insufficient. Notably, studies have indicated that higher carbon levels can enhance Charpy impact performance by stabilizing increased amounts of retained austenite (Kwok et al., 2023; Mohapatra et al., 2024b). This stabilization is correlated with favorable texture components, helping resist brittle fracture. It is also noted that excess carbon can lead to carbide networks that reduce toughness and disrupt texture uniformity, while insufficient carbon results in unstable austenite, weak γ-fiber texture, and poor transformations associated with TRIP and TWIP effects (Aliabad et al., 2025). An optimal carbon content in the range of approximately 0.2–0.3 wt% is generally preferred for automotive-grade MMnSs, providing a balance between texture sharpness and overall mechanical performance. Comparative influence of carbon content on texture evolution, retained austenite stability, and the resulting strength–ductility balance in MMnSs is shown in Table 4.

TABLE 4

Carbon levelTexture effectMicrostructural impactMechanical consequence
Low (<0.1 wt%)Weak γ-fiber, faster ferrite recrystallizationLimited retained austeniteHigher ductility, lower strength
Medium (0.15–0.3 wt%)Balanced γ-fiber and cube texturesStable retained austenite, controlled cementiteGood strength–ductility balance
High (>0.3 wt%)Strong γ-fiber, delayed recrystallizationExcess carbon segregation, risk of carbide networksHigh strength, reduced toughness

Effect of carbon content on texture evolution, retained austenite stability, and the resulting strength–ductility balance in medium-Mn steels.

4.4 Influence of aluminum (Al)

Ferrite stabilization is significantly influenced by the presence of aluminum, which acts as a strong ferrite stabilizer, counterbalancing manganese’s austenite-stabilizing effect (Sripushpa et al., 2026). This interaction effectively shifts the intercritical annealing window upwards, impacting the fraction and orientation of RA. EBSD studies have demonstrated that aluminum promotes a cube texture ({001}〈100〉) in ferrite, a feature that enhances isotropy in mechanical properties (Ridlo et al., 2025). In terms of carbide suppression, aluminum plays a crucial role by reducing cementite precipitation through the lowering of carbon activity. This suppression prevents the formation of carbide networks, resulting in cleaner grain boundaries and sharper texture components (Lin et al., 2026). Consequently, this leads to a more uniform γ-fiber ({111}) texture in austenite, thereby enhancing its ductility. Aluminum additions also affect recrystallization and annealing behavior. They delay the recrystallization of ferrite, allowing deformation textures to be preserved for longer durations (Ridlo et al., 2025). Within the temperature range of 650 °C–675 °C during intercritical annealing, aluminum-containing steels exhibit a favorable balance between strength and ductility. However, temperatures exceeding this range can destabilize austenite, resulting in martensite formation and degradation of texture. The impact of aluminum on mechanical properties is characterized by an improvement in low-temperature toughness due to grain size refinement and a shift in temper embrittlement to higher temperatures (approximately from 300 °C to 350 °C) (Lin et al., 2026). This relationship correlates with texture evolution; the refined ferrite grains with cube orientation diminish the risk of cleavage fractures. Conversely, inadequate aluminum content can lead to carbide precipitation, compromising toughness and rendering textures less stable, while excessive aluminum can excessively stabilize ferrite, reduce the amount of retained austenite, and adversely affect TRIP and TWIP effects. The optimal range of aluminum concentrations—approximately 0.2 to 0.3 wt%—strikes a balance between γ-fiber and cube textures, effectively suppresses carbides, and enhances toughness, making it particularly suited for automotive applications (Mohapatra et al., 2025a). Influence of aluminum content on texture evolution, carbide suppression, and the resulting strength–ductility balance in MMnSs is shown in Table 5.

TABLE 5

Al contentTexture effectMicrostructural impactMechanical consequence
0 wt%Strong γ-fiber, faster recrystallizationHigher carbide precipitationGood ductility, lower toughness
∼0.25 wt%Balanced γ-fiber + cube texturesSuppressed carbides, refined ferriteImproved toughness, stable retained austenite
>0.5 wt%Excess ferrite stabilization, weaker γ-fiberRisk of insufficient austenite stabilizationReduced ductility, higher brittleness

Effect of aluminum content on texture evolution, carbide suppression, and the resulting strength–ductility balance in medium-Mn steels.

4.5 Effect of silicon (Si)

Silicon plays a crucial role in inhibiting the precipitation of cementite during intercritical annealing, which allows for a higher retention of carbon in solution within the austenite phase (Mohapatra et al., 2025a). This process stabilizes the austenite and enhances the γ-fiber texture, specifically the ({111}) orientation. Improved grain boundaries resulting from Si addition lead to sharper and more uniform texture properties in the steel. By enabling the retention of carbon within austenite, Si contributes indirectly to its stabilization, which is critical for the TRIP effect. As retained austenite transforms under strain, it enhances ductility and facilitates the evolution of texture in the material. The addition of silicon delays the recrystallization of ferrite, allowing for longer preservation of deformation textures (Pierce et al., 2015). EBSD studies indicate that silicon fosters optimal cube ({001} 〈100〉) and γ-fiber textures, achieving a favorable balance between strength and ductility. In MMnSs, silicon functions synergistically with manganese (which stabilizes austenite) and aluminum (which stabilizes ferrite). This cooperative action helps control phase fractions and texture components, thereby minimizing anisotropy in mechanical properties. Notably, insufficient silicon content can lead to undesirable carbide precipitation and an unstable austenite phase, while excessive silicon can cause segregation, brittleness, and significant delays in recrystallization (Ma et al., 2026). The optimal silicon concentration is identified as being in the range of approximately 0.3–0.5 wt%, which effectively suppresses carbide formation, stabilizes austenite, and enhances the desirable γ-fiber texture for automotive-grade steel applications. Influence of silicon content on texture evolution, carbide suppression, and the resulting strength–ductility balance in MMnSs is shown in Table 6.

TABLE 6

Si contentTexture effectMicrostructural impactMechanical consequence
0 wt%Strong carbide precipitation, weaker γ-fiberReduced retained austeniteLower ductility, poor TRIP effect
∼0.2–0.5 wt%Balanced γ-fiber + cube texturesSuppressed carbides, stable austeniteGood strength–ductility balance
>1 wt%Excess suppression, delayed recrystallizationRisk of brittle phases, segregationReduced toughness, anisotropy

Impact of silicon content on texture effect, carbide suppression, and the resulting mechanical response in MMnSs.

The collective influence of Mn, Al, C, Si, and Ni on phase stability, stacking fault energy, and austenite reversion ultimately governs the strength–ductility balance that defines the performance of advanced high-strength steels. Stable and finely dispersed reverted austenite, promoted by Mn, Ni, and C, provides a sustained TRIP effect, enhancing ductility without sacrificing strength. Simultaneously, controlled reductions in SFE through Al and Si enable twinning-induced plasticity, which augments strain hardening capacity and delays necking. The synergy between these mechanisms ensures that steels can achieve high yield strength from ferritic and martensitic matrices while maintaining exceptional elongation through transformation and twinning pathways. Texture evolution further reinforces this balance, with γ-fiber strengthening improving formability and cube orientations contributing to isotropy. Thus, alloying design serves as a strategic tool to engineer microstructures that harmonize strength and ductility, positioning medium-Mn steels as a cornerstone in the development of next-generation automotive and structural materials.

5 Texture evolution associated with mechanical properties

Texture-induced anisotropy significantly influences the deep drawability and formability properties, YS, and elastic modulus of BCC steels (Xie and Nakamachi, 2002; Raabe, 1997). The properties are enhanced by the ND or γ-fiber present in the ferrite phase, whereas cleavage fractures are propagated by the (001) planes in BCC materials (Ghosh et al., 2014). Delamination behavior is adversely affected by the cube fiber texture, specifically the (001) <110> orientation (Ghosh et al., 2016). Thus, it is more advantageous to deduce from previous research that the formation of cube fibers should be limited to achieve superior tensile properties (Mohapatra et al., 2024a). The YS is reportedly enhanced when the transformation texture contains a greater proportion of fiber in the (113) <110> orientation, which is a substantial constituent of RD//<110> fiber (Hutchinson et al., 2005). Like the BCC phase, the tensile properties are significantly influenced by the textural components of the FCC phase. (Barbier et al., 2009) explained that superior tensile properties can be achieved by incorporating the texture intensities of brass components into high-manganese TWIP steel during deformation. However, MMnS exhibits distinct characteristics. The following studies examine the evolution of texture and its correlation with the tensile behavior of MMnS (Table 7).

TABLE 7

CompositionProcessing conditionsTexture componentsMechanical propertiesReferences
Fe-4.9Mn - 0.18C-0.8Si-0.4AlCR (∼73% red.) + IA 640 °C/2 h (globular) vs. Homogenization 850 °C/20 min + WQ + IA 640 °C/2 h (lamellar)Bulk texture determined for ferrite and austenite (CMWP/EBSD analysis); CMWP dislocation density calculatedYS: NA
UTS: NA
TE: NA (Study focused on EIS and potentiodynamic polarization in 3.5% NaCl)
(Kishore et al., 2023)
Fe-5Mn - 0.18C-0.80Si-0.40AlCold Rolling + IA (640 °C for 2 h); tested at Quasi-static (10–4 s-1) vs. Dynamic (200 s-1) ratesQuasi-static: Brass {110}⟨112⟩ and rotated Goss {110}⟨110⟩ in FCC; BCC {111} γ-fiber
Dynamic (200 s-1): Transitions to Copper {112}⟨111⟩, S {123}⟨634⟩, and P {011}⟨233⟩ via adiabatic heating
Quasi-static: YS ∼994 MPa, UTS ∼1,147 MPa, TE 38.8%, PSE 44.5 GPa·%
Dynamic: TE increases by ∼12% (delayed necking)
(Alam et al., 2026)
Fe-5Mn - 0.35C-3.2AlForging + Hot Rolling (880 °C, 7 mm) + Intercritical Annealing (750 °C) vs. Double IA (DIA)NA (Quantitative ODF texture components not evaluated; in situ high-energy XRD micromechanical loading partitioning and PLC bands reported)IA: UTS 777.1 MPa, TE 39.6%, PSE 30.8 GPa·%
DIA: UTS 953.6 MPa, TE 59.1%, PSE 56.4 GPa·%
YS: NA
(Mao et al., 2024)
Fe-5.6Mn - 1.1Al-0.2C and Fe-5.6Mn - 1.1Al-0.2C-0.1Ti-0.22MoHot Rolling + Cold Rolling (2 mm) + Superplastic Tensile Testing at 685 °C–775 °CODF φ2 = 45°: α-fiber (<110>//RD), weak {112}<110> and {111}<110> in α/α'; randomizes during superplastic deformation (GBS)YS: NA
UTS: NA (High-temp superplastic elongation up to 1,170% at 745 °C reported; Vickers hardness ∼280–450 HV)
(Zhang et al., 2023)
Fe-6Mn - 0.14C-0.23SiCold Rolling + Batch Annealing at 620 °C (air cooling)Pole figures {100}, {110}, {111} for ferrite and austenite (preferred orientation observed, anisotropic Lüders strain)YS: NA (Lüders strain YPE = 9.5% reported)
UTS: 1,012 MPa
TE: 42.3%
(Wang et al., 2019)
Fe-6Mn - 0.3C-3.0Al-1.5Si (IA at 760 °C)Hot rolling + Intercritical Annealing (IA) at 760 °C for 10 minUndeformed ferrite {100}⟨011⟩; post-tensile ferrite α-fiber {100} and weak γ-fiber {111}. Austenite undeformed Brass and Goss; post-tensile Brass and Cu components. Coarse δ-ferrite + UFG (α+γ) bandsYS: 788 MPa
UTS: 925 MPa
TE: 49.5%
PSE: 45.8 GPa·%
(Choi et al., 2017)
Fe-6Mn - 0.3C-3Al-1.5Si (IA at 800–880 °C)Hot rolling + IA at 800 °C, 840 °C, or 880 °C for 10 minLayered bimodal structure; higher strain-induced α′ martensite transformation (up to 73%). Ferrite/austenite ODF components as above800 °C: YS 700 MPa, UTS 985 MPa, TE 47%
840 °C: YS 700 MPa, UTS 1130 MPa, TE 35%
880 °C: YS 515 MPa, UTS 1365 MPa, TE 19.3%
(Choi et al., 2017)
Fe-6.2Mn - 0.12C-1.4Cu-0.93Ni-1.40Si (CR Route)Hot Rolling (HR) (4.3 mm) + Cold Rolling (1.5 mm) + ART Annealing (600 °C–640 °C) [Initial state: Cold-rolled martensite]FCC ODF (ϕ2 = 45°): Peak between Goss {110}⟨001⟩ and Brass {110}⟨112⟩, weak Cu {112}⟨111⟩; strong BCC γ-fiber (⟨111⟩∥ND). Nano Cu-rich particles (<20 nm), 16.8% annealing twin grainsYS: 994–1,036 MPa
UTS: 1,147–1,196 MPa
TE: 38.8%–48.5%
PSE: 44.5–58.0 GPa·%
(Yan et al., 2019)
Fe-6.83Mn - 0.22C-1.53Si (IA and Q&P Treatment)Cold rolled (1.2 mm) + Intercritical Annealing (640, 660, 680 °C for 600 s) + Quenched to 75 °C + Partitioned at 450 °C for 60 sFerrite + martensite + retained austenite (lamellar γL and equiaxed γE)
Ferrite ODF: E {111}⟨110⟩, B {011}⟨112⟩
Austenite ODF: B {011}⟨211⟩, G {110}⟨001⟩, C {112}⟨111⟩
IA640: YS ∼1,000–1,100 MPa, UTS ∼1,100 MPa, TE ∼27%
IA660: YS ∼1,180 MPa, UTS ∼1,180 MPa, TE ∼25%
IA680: YS ∼920 MPa, UTS ∼1,150 MPa, TE ∼14%
(Yang et al., 2018)
Fe-7Mn - 0.18C-4Al-1.34SiHot forging + Hot rolling (1,100 °C, 80% red.) + IA at 700 °C and 800 °C for 1 hIA _700: Strong α-fiber with dominant Brass at ∼(110); higher Cube {001}⟨100⟩ component; RA fraction ∼21.4%
IA _800: Ms Brass shifts towards Goss and Cu components; weakened Cube texture due to grain growth. RA fraction ∼32.2%
IA _700: YS: 757 MPa
UTS: 757 MPa
TE: 34%
PSE: ∼25.7 GPa·% (TRIP ratio 61%)
IA _800: YS: 771 MPa
UTS: 771 MPa
TE: 43%
PSE: ∼33.2 GPa·% (TRIP ratio 71%)
(Mohapatra et al., 2024d)
Fe-7Mn - 0.3C-3.5AlWarm Rolling (WR) + Inter critical Annealing (IA) at 775 °CQuantitative ODF components; dynamic recrystallized equiaxed dual-phase microstructure reportedYS: NA
UTS: NA
Superplastic TE: 1,401% (at 775 °C, strain rate 5 × 10−4 s-1)
(Pan et al., 2023b)
Fe-7Mn - 0.3C-3.5AlHot Rolling (80% red.) + Cold Rolling (80% red.) + HTTT at 800 °C across strain rates (5 × 10−4 to 2.5 × 10−2 s-1)5 × 10−3 s-1: Texture randomized (peak drops from 6.73 to 2.45) due to GBS dominance
2.5 × 10−2 s-1: HSRS via Rachinger sliding + DRX; 44% RA content
YS: NA
UTS: NA
Superplastic TE: 1,157% at 5 × 10−3 s-1 (m = 0.6); 322% at 2.5 × 10−2 s-1 (m = 0.43)
PSE: NA
(Pan et al., 2023c)
Fe-7.23Mn - 0.09C-4.42Al-1.99Si-0.5Cu (A0: 0% pre-strain)
Fe-7.23Mn - 0.09C-4.42Al-1.99Si-0.5Cu (A2: 2% pre-strain)
HR + Annealing (750 °C, 5 h) + CR (1.5 mm) + 0% pre-strain + Q and P (750 °C 20 min → 25 °C 90s → WQ)Multiphase martensite, α-ferrite, δ-ferrite, retained austenite. Higher ⟨111⟩ texture, lower ⟨001⟩ and ⟨101⟩. Lath-like retained austenite
Refined multiphase structure; stronger ⟨111⟩ and ⟨101⟩ orientations. 73.8% large-angle grain boundaries. Blocky/granular retained austenite stabilized by C/Mn
YS: NA
UTS: 896 MPa
TE: 34.72%
PSE: 31.10 GPa·%
YS: NA
UTS: 902 MPa
TE: 39.28%
PSE: 35.43 GPa·%
(Wu et al., 2023)
Fe-9.35Mn - 0.22C-7.19Al-1.12Si-0.03Ti (A2: Ti-modified)
Fe-9.80Mn - 0.2C-7.50Al-1.22Si (A1: Ti-free)
Forged + HR + CR (50% red. to 2 mm) + Salt bath annealed at 1073 K (800 °C) for 3 min or 50 minDuplex ferrite + austenite with Ti-rich intermetallic carbides (∼15–35 nm) + Mn5(Si,Al)C. Ferrite γ-fiber and Cube fiber evolution governed by Taylor factor M distribution (∼2–5)
Ti free
Duplex ferrite + austenite with Mn5(Si,Al)C precipitates (150–300 nm)
Ferrite ODF: γ-fiber ({111}⟨110⟩ to {111}⟨112⟩), Cube fiber ({001}⟨110⟩ to {001}⟨010⟩)
Austenite ODF: α-fiber (Goss to Brass)
A2-3min: YS ∼880 MPa, UTS ∼1,020 MPa, TE ∼18%
A2-50min: YS ∼870 MPa, UTS ∼980 MPa, TE ∼28%
A1-3min: YS ∼910 MPa, UTS ∼1,130 MPa, TE ∼25%
A1-50min: YS ∼810 MPa, UTS ∼920 MPa, TE ∼12%
(Sarkar et al., 2019)
Fe-10.86Mn - 2.2Al-1.8Si-0.22C60% Cold Rolling + Intercritical Annealing (800 °C for 30 min)Residual <101> austenite texture retained after CR; orientation randomization increases after IA with decrease in K-S relationshipYS: NA
UTS: NA
TE: NA (PSE ≥60 GPa·% cited; in-situ EBSD grain refinement mechanisms)
(Liu et al., 2025)
Fe-11.2Mn - 0.2C-1.95AlCold rolling (1 mm) + Controlled Annealing (600 °C–750 °C, 5 min–48 h)Ferrite grains with strong γ-fiber ({111}∥ND) and α-fiber. γ-fiber intensity increases with soaking timeYS: ∼600–880 MPa
UTS: ∼1,000–1,350 MPa
TE: >30%
PSE: >30 GPa·% (Yield Point Elongation YPE suppressed via γ-fiber)
(Cai et al., 2019)

Showing MMnS compositions and processing conditions versus texture components and mechanical properties.

5.1 Effect of annealing temperature

It was reported that α-fiber in the FCC phase remains unchanged after the tensile deformation in intercritically annealed Fe-6.78Mn-3.92Al-0.18C (wt%) MMnS samples (Mohapatra et al., 2023e). The orientation distribution function (ODF) represents the texture components of the samples. The pre-tensile ODFs of A_700, A_750, and A_800 samples (annealed at 700, 750, and 800 °C, respectively) are displayed in Figure 4. More recrystallization and independent orientations resulted from decreased textural-component intensity as annealing temperature increased. All the annealed samples exhibit significant α-fiber, resulting in randomly oriented grains and reduced cube components (Mohapatra et al., 2024c).

FIGURE 4

All the deformed samples have substantial α-fiber components, notably Ms brass and Goss/brass twin (Figure 5). Deformed samples have strong Cu and S components. Nevertheless, the primary constituent of the texture, Ms brass {011} 〈211〉, partially shifted towards the Goss/brass twin {011} 〈111〉 component, exhibiting the TRIP effect when subjected to tensile deformation.

FIGURE 5

5.2 Effect of cold rolling on texture

Figure 6 illustrates the initial microstructures of the experimental cold-rolled (CR) steel before tensile deformation. Red and green contrasts, respectively, represent the BCC and FCC phases. White and black lines indicate low-angle grain boundaries (LAGBs) (2°–15°) and high-angle grain boundaries (HAGBs) (≥15°), respectively (Figure 6a). The microstructures of the CR steel primarily consist of α′ martensite, along with a small fraction of retained γ austenite grains (Figure 6a). The average grain size is approximately 0.88 μm. The CR process has introduced a significant amount of deformation energy storage within the microstructure (Figure 6b). Approximately 67% of the grain boundaries are LAGBs, a result of the extensive deformation experienced during the CR process. Furthermore, the ODF indicates that the BCC phase exhibits a strong α-fiber orientation along the rolling direction (RD), with a maximum orientation strength of 5.40 (Figure 6c). In contrast, the FCC phase shows a strong {110} orientation with a maximum orientation strength of 17.90 (Figure 6d).

FIGURE 6

Based on the above tensile results, the samples at the typical temperatures of 700 °C and 750 °C with a true strain of 0.2 were selected to conduct microstructure characterization. The γ content is about 16.7% at 700 °C and 22.2% at 750 °C, which is almost the same when the true strain is 0.9 (Figures 7, 8). This implies that the samples have been completely austenitized before the jump test. During deformation at 700 °C, the average grain size increased by 0.13 μm at 0.9 true strain compared to the initial cold-rolled sheet. Moreover, Figure 7c,d shows that the BCC and FCC phases have distinct textures. It is clear that the initial texture intensity of the two phases is distinct, indicating a change in orientation during deformation. The α-fiber of the BCC phase is enhanced, and the FCC phase is transformed into the brass texture. A change in grain orientation can demonstrate that at high temperatures, materials with such fine microstructure undergo GBS.

FIGURE 7

FIGURE 8

Figure 8 illustrates that at a true strain of 0.9 °C and 750 °C, the microstructure of experimental samples underwent significant transformation, with numerous BCC phases converting into FCC phases, leading to an increase in average grain size from 1.01 μm to 1.31 μm. The FCC phase exhibited classic deformation characteristics, with key mechanisms including dynamic recovery and associated fiber evolution from α-fiber {001} to γ-fiber {111}. The FCC phase also developed a brass texture with a maximum orientation strength of 5.72, while {112} nearly vanished, indicating strong superplasticity in the γ-fiber and brass textures (Pan et al., 2023a; Razmpoosh et al., 2020).

5.3 Influence of strain rate on evolution of texture

The influence of strain rate on texture evolution in intercritically annealed Fe-6.78Mn-3.92Al-0.18C (wt%) MMnS has been recently studied (Mohapatra et al., 2023f). A high TRIP effect and austenite transformation ratio (ratio of martensite transformed from austenite during tensile deformation) resulted in a higher low-angle grain boundary (LAGB) fraction in the strained Fe-6.78Mn-3.92Al-0.18C (wt%) steel at lower strain rates (1.33 × 10−4 s-1) (Mohapatra et al., 2025b). Ms brass {011} 〈211〉 facilitates the TRIP effect more than other textural components at lower strain rates (1.33 × 10−4 s-1) (Figure 9).

FIGURE 9

Recently, researchers investigated the evolution of mesotexture (Patra et al., 2024) specifically focusing on the misorientation angle and axis during the strain-induced martensite transformation under various deformation conditions (Figure 10). The transformation from austenite to α′ martensite adheres to specific crystallographic orientation relationships (OR), particularly the Kurdjumov–Sachs (K–S) type, which is characterized by a misorientation angle of 42.8° around the orientation. Deformations can disrupt the ideal K–S orientation due to grain rotations. Analyzing the distributions of misorientation angles in the deformed samples reveals a consistent and prominent peak at approximately 42.8° across all deformation conditions, indicating successful strain-induced formation of α′ martensite. Samples subjected to a deformation rate of 10–3 s-1 at room temperature exhibit a sharper peak at this angle with a higher frequency compared to other conditions, suggesting a greater proportion of retained austenite transforming under strain, thus promoting K–S boundary formation. Conversely, at elevated temperatures (409 K) and higher strain rates, the saturation of phase transformation leads to grain rotation, which is necessary to accommodate the deformation, resulting in a deviation from the expected misorientation angle.

FIGURE 10

Overall, this analysis confirms the crucial influence of deformation parameters on martensitic transformation processes. The sample, which deformed at a strain rate of 10–3 s-1 at room temperature, exhibits a pronounced peak at 42.8°. This peak is sharper and occurs at a higher frequency compared to other deformation conditions. This phenomenon is attributed to an increased fraction of retained austenite undergoing strain-induced transformation, resulting in boundaries characterized by K–S orientation relationships (OR). Conversely, under conditions of higher strain rates or elevated temperatures, particularly at 409 K, phase transformation reaches saturation. This saturation leads to grain rotation to accommodate deformation, causing deviations from the ideal misorientation angle. Apart from the observed deviation in the misorientation angle, significant changes in the misorientation axis have been recorded during deformation at elevated strain rates. The analysis of the evolution of the misorientation axis with respect to the plastic strain (εp) in samples subjected to a strain rate of 10–3 s-1, as illustrated in Figure 11a, reveals a notable peak near the direction. This peak intensifies with increasing values of εp. Conversely, the results presented in Figure 11b indicate that for samples deformed at a higher strain rate of 103 s-1, the misorientation axis not only shifted towards the [001] direction as εp increased but also exhibited a close correlation with the saturation of the phase transformation. This suggests a significant relationship between the evolution of the misorientation axis and the deformation conditions in high strain rate scenarios.

FIGURE 11

The standard ODF section at φ2 = 45° is illustrated in Figure 12a, highlighting important texture components for the BCC phase. The experimental micro-textures for hot-forged (HF) and hot-rolled (HR) specimens are shown in Figures 12b,c, respectively, while the corresponding simulated micro-textures are depicted in Figures 12d,e. The HF specimen exhibits high-intensity Goss {110} and cube texture {001}, with a relatively weaker intensity of {111} also visible in the ODF section at φ2 = 45° (Figure 12b). In contrast, the HR specimen features a rotated-cube texture {001} accompanied by a significantly weakened cube texture {001} (Figure 12c). A comparison between Figures 12b,c reveals that the intensity of the γ-fiber {111}//ND is notably higher in the HR specimen compared to the HF specimen, indicating a difference in micro-textural characteristics.

FIGURE 12

Moreover, to investigate the influence of strain rates on deformation mechanisms, pole figures for deformed samples are presented (Figure 13). At a strain of ε = 0.2, samples exhibit a similar rolling texture, with peak densities ranging from 6.35 to 6.75. At a strain rate of 5 × 10−4 s-1 and ε = 0.8, the texture becomes more concentrated with a peak density of 9.56, suggesting that dislocation slip may be the primary mechanism of deformation. Following significant dislocation slip and creep, small dimensions nucleate and recrystallize. In fractured samples, the peak density drops to 5.46, revealing peaks in multiple directions due to the continuous generation of fine grains, which enhances grain boundary sliding (GBS). At a higher strain rate of 5 × 10−3 s-1, as the strain progresses from ε = 0.8 to fracture, peak density decreases from 6.73 to 2.45, leading to a nearly random texture distribution and indicating that GBS predominantly governs superplastic deformation under these conditions. The behavior at 5 × 10−3 s-1 mirrors the previous trend, though the amplitude of variation is slightly less pronounced, further confirming the key role of GBS in high strain rate superplasticity in multi-phase materials.

FIGURE 13

5.4 Texture associated with fracture characteristics

It is also found that the transverse fracture in intercritically annealed Fe-6.78Mn-3.92Al-0.18C (wt%) MMnS exhibits a higher degree of propagation along the 〈101〉 direction as a result of its lower relative intensity (Mohapatra et al., 2024d). Figure 14 shows inverse pole figure (IPF) maps of the (a) BCC and (b) FCC phases, together with the corresponding IPF texture maps of the (c) BCC and (d) FCC phases, obtained from the tensile-tested IA750 sample near the fracture surface. The BCC grains exhibit pronounced crack propagation and arrest along {111} orientations, reflected in the strong texture intensities. In contrast, the FCC phase shows smoother crack paths and a broader orientation distribution, consistent with enhanced slip and twinning activity. In the FCC phase, most RA grains are oriented along the 〈101〉 direction, while a smaller number are distributed between the 〈101〉 and 〈111〉 directions. The combined analysis highlights the distinct deformation and fracture responses of the two phases, underscoring their complementary roles in strength–ductility balance.

FIGURE 14

6 Overview of the review work

The rotation and orientation of grains following deformation significantly affect the mechanical properties of steel, as the crystallographic texture plays a crucial role in influencing mechanical anisotropy (Kumar et al., 2025b). In crystallography, the texture is represented as {HKL}. For rolled steel sheets, this notation indicates the orientation of crystal planes that align with the rolling plane (RP) and the rolling direction (RD). Key deformation textures include α-fibers, ε-fibers, and γ-fibers, which are associated with specific fiber axes along the RD, transverse direction (TD), and normal direction (ND), respectively (Nafisi et al., 2012). The {332} component is known for optimally balancing strength and toughness, while the {113} and {112} textures tend to increase mechanical anisotropy (Ray and Jonas, 1990). Observations indicate the development of {100}, {113}, and {332} textures across different thermomechanical processing routes, with the {332} and {113} components arising from orientations found in deformed austenite (Venkatsurya et al., 2013). It was noticed that the primary deformation textures in X70 and X80 pipeline steels are the α-fiber (//RD), γ-fiber (//ND), and ε-fiber (//TD). The {112}, {113}, and {223} components contribute to the anisotropy in YS (Venkatsurya et al., 2012). The orientation of neighboring grains plays a significant role in crack propagation (Baczynski et al., 1999). Specifically, {001} planes increase the risk of brittle fracture, while grains with a {001}//normal plane (NP) orientation decrease transgranular and intergranular low-resistance paths (Wright and Field, 1998). This reduction leads to crack coalescence and stepwise hydrogen-induced cracking. Conversely, {111}//NP textures foster high-resistance intergranular crack paths. Furthermore, {001} planes act as primary pathways for transgranular cleavage, which can result in sudden brittle failure when aligned with the fracture surface. It was found that emphasized that grains textured with the {111}//rolling plane can reduce crack propagation in steels (Razmpoosh et al., 2020). Numerous studies have examined the influence of thermo-mechanical control rolling parameters on crystallographic texture and microstructure, particularly drawing attention to the importance of finish rolling temperature in achieving deformation texture in low-alloy steel (Omale et al., 2017). Lower temperatures promote the {111} texture, whereas higher temperatures result in diminished intensity (Guo et al., 2008). Furthermore, the development of a cube ({100}) texture is linked to a decrease in the tensile properties of medium-Mn steel, as the {100} plane functions as a cleavage plane in BCC materials (Wang et al., 2022). Conversely, grains aligned in the {111} and {110} directions enhance ductility and tensile properties, leading to improved strength due to the formation of γ-fiber {111}//ND and brass {110} textures through thermo-mechanical processing (Pan et al., 2023a). However, the precise effect of these textures on crack susceptibility remains unclear. Texture evolution is critically important for determining mechanical properties, particularly the stability of austenite against martensitic transformation, which is influenced by the crystal orientation in relation to applied stress (Yan et al., 2018). During the martensitic transformation, the selection of variants impacts texture; however, mechanisms such as crystal rotation and twinning also contribute significantly (Wang et al., 2014). Recent studies suggest that the rotation of austenite during deformation improves the ductility of traditional TRIP steels by serving as a barrier to dislocation movement, thereby delaying the onset of crack formation (Tirumalasetty et al., 2012). Observations made during tensile testing reveal increased intensity in certain orientations of austenite and martensitic structures, indicating a stress-assisted transformation (Morales-Rivas et al., 2018). This suggests that both stress and the accommodation of martensite twins play vital roles in texture development, extending beyond mere interactions between stress direction and shape change strain. Comparative overview of ferritic, austenitic, and duplex medium-Mn steels, highlighting Mn range, dominant phases, texture components, operative mechanisms, and their mechanical implications is shown in Table 8. In addition, Table 9 shows the influence of key alloying elements (Mn, Ni, C, Al, Si) on phase stability, stacking fault energy, austenite reversion, and texture development in medium-Mn steels.

TABLE 8

MMnS
Class
Mn rangeDominant phasesTexture componentsMechanismsMechanical implications
Ferritic3–6 wt%α-ferrite + minor γCube, α-fiber, weak γ-fiberSlip, limited TRIPHigh strength, limited ductility
Austenitic9–12 wt%γ-austeniteStrong γ-fiber, {111}, {110}TWIP, slipExceptional ductility, moderate strength
Duplex6–9 wt%Ferrite + γ-austeniteCube, α-fiber, strong γ-fiberTRIP + TWIP synergyOptimal strength–ductility balance

Classification of medium-Mn steels (ferritic, austenitic, duplex) with Mn range, dominant phases, texture components, operative mechanisms, and mechanical implications.

TABLE 9

ElementPhase stabilitySFE effectAustenite reversionTexture contribution
Mnγ-stabilization↑ SFEAccelerates reversionStrengthens γ-fiber
Niγ- stabilization↑ SFEStabilizes reverted γStrengthens γ-fiber
Cγ stabilization↑ SFEAccelerates reversionStrengthens γ-fiber
AlFerrite stabilization↓ SFERetards reversionPromotes cube, twinning reorientation
SiSuppresses carbides↓ SFEAids reversionFacilitates twinning, strengthens {111}

Comparative summary of the influence of alloying elements.

7 Research gaps, challenges, and perspectives

The research on MMnSs faces several unresolved challenges that intersect various domains. Current predictive models are unable to accurately represent the complex interplay between TRIP and TWIP under industrial conditions. Additionally, dynamic processes such as austenite reversion and twinning have not been thoroughly explored due to limited in situ characterization techniques. Findings related to texture control from laboratory experiments require further validation through pilot-scale trials to ensure that they can be scaled effectively for industrial applications. The understanding of corrosion-mechanical coupling is notably inadequate, with a particular lack of insight into how grain boundary character distribution affects long-term performance of the steels. Moreover, welding and joining processes often lead to the degradation of the γ fiber in heat-affected zones, which compromises the mechanical integrity of the materials. Furthermore, alloy design is hindered by a lack of systematic frameworks for optimizing combinations of manganese, nickel, carbon, aluminum, and silicon, while the fatigue performance of these steels under cyclic loading conditions has not been sufficiently researched. Collectively, these gaps underscore the pressing need for integrated modeling approaches, advanced real-time characterization methods, scalable processing strategies, and comprehensive evaluations of service performance to advance the field of MMnSs. Future research must integrate advanced characterization and predictive modeling to bridge laboratory findings with industrial processing, ensuring MMnSs fulfill their potential as next-generation automotive steels.

8 Conclusion

This review highlights that texture development in medium-Mn steels is intrinsically linked to their phase constitution, alloying chemistry, and thermomechanical processing. The following are the conclusions derived from the current review of texture development in medium manganese steel.

  • Medium-Mn steels are advanced high-strength steels characterized by the interaction of phase constitution, texture evolution, and deformation mechanisms. Ferritic grades, primarily composed of α-ferrite, offer high yield strength and stability but have limited ductility, relying on the TRIP effect. Austenitic grades, with increased Mn and Ni, provide outstanding ductility through the TWIP effect, though they sacrifice some strength and increase costs. Duplex steels, which balance ferrite and austenite, combine TRIP and TWIP effects, resulting in beneficial strength-ductility combinations and mechanical isotropy.

  • The roles of alloying elements are crucial: Mn stabilizes γ-fiber and supports the TRIP/TWIP mechanisms; Ni improves grain refinement and slip/twinning; carbon (C) stabilizes retained austenite and influences texture; aluminum (Al) suppresses carbide formation and promotes cube textures in ferrite; while silicon (Si) enhances austenite stability and reduces anisotropy. Precise control over these elements is essential, as imbalances can adversely affect toughness, corrosion resistance, and texture consistency.

  • Processing conditions, including intercritical annealing temperatures, cold rolling, and thermomechanical treatments, significantly influence the texture evolution and mechanical behavior of the steels. The transitions among various orientations (cube, α-fiber, brass, γ-fiber) illustrate the sensitivity of Medium-Mn steels to strain paths and thermal histories, highlighting the necessity for predictive models that incorporate alloy composition, phase transformation kinetics, and texture development.

  • Ultimately, Medium-Mn steels provide a customizable framework for achieving optimal strength-ductility relationships through deliberate microstructural design and texture engineering. They are particularly valuable for automotive and structural applications, where safety and formability are critical. Future research should focus on integrated alloy design, advanced characterization techniques, and process optimization to fully exploit the capabilities of Medium-Mn steels while addressing challenges related to cost, segregation, and corrosion resistance.

Statements

Author contributions

SM: Conceptualization, Data curation, Formal Analysis, Investigation, Methodology, Supervision, Writing – original draft, Writing – review and editing. RP: Formal Analysis, Writing – review and editing. BM: Formal Analysis, Writing – review and editing. PS: Writing – review and editing.

Funding

The author(s) declared that financial support was received for this work and/or its publication. Authors thank the OUTR, Bhubaneswar, for the support.

Conflict of interest

The author(s) declared that this work was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.

Generative AI statement

The author(s) declared that generative AI was not used in the creation of this manuscript.

Any alternative text (alt text) provided alongside figures in this article has been generated by Frontiers with the support of artificial intelligence and reasonable efforts have been made to ensure accuracy, including review by the authors wherever possible. If you identify any issues, please contact us.

Publisher’s note

All claims expressed in this article are solely those of the authors and do not necessarily represent those of their affiliated organizations, or those of the publisher, the editors and the reviewers. Any product that may be evaluated in this article, or claim that may be made by its manufacturer, is not guaranteed or endorsed by the publisher.

References

  • 1

    AlamM. I.WippS.ChandanA. K.MishraG.ShekharS.BleckW.et al (2026). Strain rate dependent deformation behavior evolution and ensuing tensile properties of a medium manganese steel. Mater. Sci. Eng. A972, 150587. 10.1016/j.msea.2026.150587

  • 2

    AliabadR. S.SadeghpourS.KarjalainenP.KömiJ.SinghH.JavaheriV. (2025). Carbon redistribution in a martensitic medium Mn steel during heating to intercritical region: an in-situ synchrotron XRD study. Procedia Struct. Integr.69:69–75. 10.1016/j.prostr.2025.07.010

  • 3

    BaczynskiG. J.JonasJ. J.CollinsL. E. (1999). The influence of rolling practice on notch toughness and texture development in high-strength linepipe. Metall. Mater. Trans. A30, 3045–3054. 10.1007/s11661-999-0215-5

  • 4

    BaiS.XiaoW.NiuW.LiangW. (2021). Microstructure and mechanical properties of a medium-mn steel with 1.3 gpa-strength and 40%-ductility. Mater. (Basel)14, 2233. 10.3390/ma14092233

  • 5

    BarbierD.GeyN.AllainS.BozzoloN.HumbertM. (2009). Analysis of the tensile behavior of a TWIP steel based on the texture and microstructure evolutions. Mater. Sci. Eng. A500, 196–206. 10.1016/j.msea.2008.09.031

  • 6

    BhadeshiaHKDH (2005). High performance bainitic steels. Mater. Sci. Forum500–501, 63–74. 10.4028/0-87849-981-4.63

  • 7

    CaiM.LiZ.ChaoQ.HodgsonP. D. (2014). A novel Mo and Nb microalloyed medium Mn TRIP steel with maximal ultimate strength and moderate ductility. Metall. Mater. Trans. A Phys. Metall. Mater. Sci.45, 5624–5634. 10.1007/s11661-014-2504-x

  • 8

    CaiZ. H.CaiB.DingH.ChenY.MisraR. (2016). Microstructure and deformation behavior of the hot-rolled medium manganese steels with varying aluminum-content. Mater. Sci. Eng. A676, 263–270. 10.1016/j.msea.2016.08.119

  • 9

    CaiZ. H.JingS. Y.LiH. Y.ZhangK.MisraR.DingH.et al (2019). The influence of microstructural characteristics on yield point elongation phenomenon in Fe-0.2C-11Mn-2Al steel. Mater. Sci. Eng. A739, 17–25. 10.1016/j.msea.2018.09.114

  • 10

    CapekJ.CernikM.GanevN.TrojanK.NemecekJ.KolarikK. (2018). Comparison of rolling texture of austenite and ferrite phases of duplex steel with single-phase austenitic and ferritic steel. IOP Conf. Ser. Mater. Sci. Eng.375, 012025. 10.1088/1757-899X/375/1/012025

  • 11

    CenQ.WangW.ZhangB.YanZ.WangY.ZhangM. (2022). Influence of Ni addition on the microstructure and mechanical properties of 3.5Mn Medium-Mn steel. Metall. Mater, Trans. A Phys. Metall. Mater, Sci.53, 4034–4046. 10.1007/s11661-022-06808-w

  • 12

    ChenS.RanaR.HaldarA.RayR. K. (2017). Current state of Fe-Mn-Al-C low density steels. Prog. Mater. Sci.89, 345–391. 10.1016/j.pmatsci.2017.05.002

  • 13

    ChengP.HuB.LiuS. L.GuoH.EnomotoM.ShangC. (2019). Influence of retained austenite and Cu precipitates on the mechanical properties of a cold-rolled and intercritically annealed medium Mn steel. Mater, Sci. Eng. A746, 41–49. 10.1016/j.msea.2018.12.111

  • 14

    ChoiH.LeeS.LeeJ.BarlatF.De CoomanB. C. (2017). Characterization of fracture in medium Mn steel. Mater, Sci. Eng. A687, 200–210. 10.1016/j.msea.2017.01.055

  • 15

    DaiZ.DingR.YangZ.ZhangC.ChenH. (2018). Thermo-kinetic design of retained austenite in advanced high strength steels. Acta Mater,152, 288–299. 10.1016/j.actamat.2018.04.040

  • 16

    DalaiR.MohapatraS.DasS.DasK. (2023). Effect of thermo – processing on the microstructure, impact abrasion wear, and corrosion resistance properties of TiC reinforced Al-Added High-Mn steel matrix composite. JOM75, 5281–5289. 10.1007/s11837-023-05974-5

  • 17

    DalaiR. P.MohapatraS.PadhyA.PradhanR. (2026). Influence of annealing temperature on the microstructure and tensile properties of hot-rolled high-C, high-Mn steel. Mater. Lett.424:141525. 10.1016/j.matlet.2026.141525

  • 18

    De CoomanB. C.KwonO.ChinK. G. (2012). State-of-the-knowledge on TWIP steel. Mater. Sci. Technol.28, 513–527. 10.1179/1743284711Y.0000000095

  • 19

    DuttaA.PongeD.SandlöbesS.RaabeD. (2019). Strain partitioning and strain localization in medium manganese steels measured by in situ microscopic digital image correlation. Materialia5, 100252. 10.1016/j.mtla.2019.100252

  • 20

    GhoshA.KunduS.ChakrabartiD. (2014). Effect of crystallographic texture on the cleavage fracture mechanism and effective grain size of ferritic steel. Scr Mater.81, 8–11. 10.1016/j.scriptamat.2014.02.007

  • 21

    GhoshA.PatraS.ChatterjeeA.ChakrabartiD. (2016). Effect of local crystallographic texture on the fissure formation during charpy impact testing of low-carbon steel. Metall. Mater. Trans. A Phys. Metall. Mater. Sci.47, 2755–2772. 10.1007/s11661-016-3458-y

  • 22

    GrajcarA.KilarskiA.KozlowskaA. (2018). Microstructure–property relationships in thermomechanically processed medium-Mn steels with high Al content. Met. (Basel)8, 1–19. 10.3390/met8110929

  • 23

    GuoY.WangZ.ZouW.LiuX. h.WangG. d. (2008). Textures and properties of hot rolled high strength Ti-IF steels. J. Iron Steel Res. Int.15, 70–76. 10.1016/S1006-706X(08)60252-6

  • 24

    HanY.ShiJ.XuL.CaoW.DongH. (2011). TiC precipitation induced effect on microstructure and mechanical properties in low carbon medium manganese steel. Mater. Sci. Eng. A530, 643–651. 10.1016/j.msea.2011.10.037

  • 25

    HanJ.da SilvaA. K.PongeD.RaabeD.LeeS. M.LeeY. K.et al (2017). The effects of prior austenite grain boundaries and microstructural morphology on the impact toughness of intercritically annealed medium Mn steel. Acta Mater.122:199–206. 10.1016/j.actamat.2016.09.048

  • 26

    HuB.LuoH.YangF.DongH. (2017). Recent progress in medium-Mn steels made with new designing strategies, a review. J. Mater. Sci. Technol.33, 1457–1464. 10.1016/j.jmst.2017.06.017

  • 27

    HuB.HeB. B.ChengG. J.YenH.HuangM.LuoH. (2019). Super-high-strength and formable medium Mn steel manufactured by warm rolling process. Acta Mater.174, 131–141. 10.1016/j.actamat.2019.05.043

  • 28

    HuC.HuangC. P.LiuY. X.PerladeA.ZhuK.HuangM. (2023). The dual role of TRIP effect on ductility and toughness of a medium Mn steel. Acta Mater.245, 118629. 10.1016/j.actamat.2022.118629

  • 29

    HuiW.ShaoC.ZhangY.ZhaoX.WengY. (2017). Microstructure and mechanical properties of medium Mn steel containing 3%Al processed by warm rolling. Mater. Sci. Eng. A707, 501–510. 10.1016/j.msea.2017.09.090

  • 30

    HutchinsonB.RydeL.BateP. (2005). Transformation-textures in steels. Mater. Sci. Forum495–497, 1141–1150. 10.4028/0-87849-975-x.1141

  • 31

    JacobR.Raman SankaranarayananS.Kumaresh BabuS. P. (2019). “Recent advancements in manganese steels-A review,” in Materials Today: Proceedings (Elsevier Ltd), 2852–2858.

  • 32

    JiaN. N.GuoK.HeY. M.WangY.PengJ.WangT. (2017). A thermomechanical process to achieve mechanical properties comparable to those of quenched-tempered medium-C steel. Mater. Sci. Eng. A700, 175–182. 10.1016/j.msea.2017.06.011

  • 33

    KishoreK.ChandanA. K.PurtyM.KarthikV.MishraG.Kumar SahooB.et al (2023). Effect of microstructure on corrosion behavior of medium manganese steel. Mater Lett.330, 133344. 10.1016/j.matlet.2022.133344

  • 34

    KumarS.RakshitR.PrasadA. D.JayabalanB.MukherjeeS.MandalS. (2023). Excellent strength-ductility synergy in a novel medium manganese steel containing 2.4Al-2.9Mn-4.1Ni realized through limited thermo-mechanical processing steps. Mater, Sci. Eng. A883, 145488. 10.1016/j.msea.2023.145488

  • 35

    KumarS.GhoshD.RakshitR.MukherjeeS.MandalS. (2025a). Unveiling the correlation among microstructure, texture, slip system activity, and tensile property in a hot rolled Ni containing Medium Mn steel. Steel Res. Int.96:2400537. 10.1002/srin.20400537

  • 36

    KumarS.GhoshD.RakshitR.MukherjeeS.MandalS. (2025b). Unveiling the correlation among microstructure, texture, slip system activity, and tensile property in a hot rolled Ni containing Medium-Mn steel. Steel Res. Int.96, 2400537. 10.1002/srin.202400537

  • 37

    KwokT. W. J.WorsnopF. F.DouglasJ. O.DyeD. (2023). Carbon in solution and the charpy impact performance of medium Mn steels. Metall. Mater, Trans. A54, 4128–4137. 10.1007/s11661-023-07157-y

  • 38

    LamariM.GeandierG.NakonechnaO.PerladeA.ZhuK.AllainS. (2026). In situ quantification of cementite precipitation/dissolution kinetics and austenite carbon enrichment in medium Mn steels. Mater, Des.265:115966. 10.1016/j.matdes.2026.115966

  • 39

    LeeY. K.HanJ. (2015). Current opinion in medium manganese steel. Mater, Sci. Technol. (United Kingdom)31, 843–856. 10.1179/1743284714Y.0000000722

  • 40

    LeeS.EstrinY.De CoomanB. C. (2013). Constitutive modeling of the mechanical properties of V-added medium manganese TRIP steel. Metall. Mater, Trans. A Phys. Metall. Mater. Sci.44, 3136–3146. 10.1007/s11661-013-1648-4

  • 41

    LeeH.JoM. C.SohnS. S.ZargaranA.RyuJ. H.KimN. J.et al (2018). Novel medium-Mn (austenite + martensite) duplex hot-rolled steel achieving 1.6 GPa strength with 20 % ductility by mn-segregation-induced TRIP mechanism. Acta Mater147, 247–260. 10.1016/j.actamat.2018.01.033

  • 42

    LiZ. C.MisraR. D. K.CaiZ. H.LiH.DingH. (2016). Mechanical properties and deformation behavior in hot-rolled 0.2C-1.5/3Al-8.5Mn-Fe TRIP steel: the discontinuous TRIP effect. Mater. Sci. Eng. A673, 63–72. 10.1016/j.msea.2016.07.023

  • 43

    LiZ. C.DingH.MisraR. D. K.CaiZ. H. (2017a). Microstructure-mechanical property relationship and austenite stability in medium-Mn TRIP steels: the effect of austenite-reverted transformation and quenching-tempering treatments. Mater. Sci. Eng. A682, 211–219. 10.1016/j.msea.2016.11.048

  • 44

    LiY.LiW.MinN.LiuW.JinX. (2017b). Effects of hot/cold deformation on the microstructures and mechanical properties of ultra-low carbon medium manganese quenching-partitioning-tempering steels. Acta Mater.139, 96–108. 10.1016/j.actamat.2017.08.003

  • 45

    LiX.SongR.ZhouN.LiJ. (2018a). Microstructure and tensile behavior of Fe-8Mn-6Al-0.2C low density steel. Mater. Sci. Eng. A709, 97–104. 10.1016/j.msea.2017.10.039

  • 46

    LiX.SongR.ZhouN.LiJ. (2018b). An ultrahigh strength and enhanced ductility cold-rolled medium-Mn steel treated by intercritical annealing. Scr Mater.154, 30–33. 10.1016/j.scriptamat.2018.05.016

  • 47

    LiQ.SunY.ZuoH.FengJ.LiZ.CaiZ.et al (2024). Microstructure evolution and mechanical properties of light medium manganese steel: different rolling directions during warm stamping. J. Mater. Eng. Perform.33, 13882–13896. 10.1007/s11665-023-08998-9

  • 48

    LinZ.ZhouW.HuC.ZhangS. l.HuF.XuK.et al (2026). Effect and mechanism of Al content on the microstructure and low-temperature impact toughness of warm-rolled and tempered medium-Mn steels. J. Mater. Res. Technol.43:3590–3602. 10.1016/j.jmrt.2026.06.303

  • 49

    LiuL.HeB.HuangM. (2018). The role of transformation-induced plasticity in the development of advanced high strength steels. Adv. Eng. Mater.20, 1701083. 10.1002/adem.201701083

  • 50

    LiuS.ZhangM.LiuZ.JinM.ChenL.CaiX.et al (2025). The study of austenite reverse transformation and grain refinement mechanisms in medium manganese steel during intercritical annealing process. Mater. Charact.227, 115345. 10.1016/j.matchar.2025.115345

  • 51

    LuoL.LiW.WangL.ZhouS.JinX. (2017). Tensile behaviors and deformation mechanism of a medium Mn-TRIP steel at different temperatures. Mater. Sci. Eng. A682, 698–703. 10.1016/j.msea.2016.11.017

  • 52

    MaY.SunB.SchökelA.SongW.PongeD.RaabeD.et al (2020). Phase boundary segregation-induced strengthening and discontinuous yielding in ultrafine-grained duplex medium-Mn steels. Acta Mater.200, 389–403. 10.1016/j.actamat.2020.09.007

  • 53

    MaC.WangJ.MaY.JiaoF.JiaQ.ZhangL.et al (2026). Silicon-dictated strain-hardening behavior and fracture resistance in 1300 MPa-grade medium Mn steels. Mater. Charact.232, 116026. 10.1016/j.matchar.2026.116026

  • 54

    MandalA. (2016). Processing-Microstructure-Microtexture-Property Correlation of Duplex Stainless Steels, 1–194.

  • 55

    MaoP. N.LiuJ. J.HuangX. M.ZhongZ.ZhangJ.ShiY. (2024). The effect of double intercritical annealing on micromechanical behavior of a medium Mn transformation induced plasticity steel investigated by in situ high energy X-ray diffraction. Mater. Sci. Eng. A902, 146576. 10.1016/j.msea.2024.146576

  • 56

    MishraG.ChandanA. K.KunduS. (2017). Hot rolled and cold rolled medium manganese steel: mechanical properties and microstructure. Mater. Sci. Eng. A701, 319–327. 10.1016/j.msea.2017.06.088

  • 57

    MohapatraS. K. (2023). Development of Aluminum Added Medium Manganese Steel for Automotive Applications.

  • 58

    MohapatraS.DasK.DasS. (2022). Effect of annealing time on the microstructure and mechanical properties of aluminum added low-density medium manganese steel. Mater. Lett.318, 132211. 10.1016/j.matlet.2022.132211

  • 59

    MohapatraS.KumarS.DasS.DasK. (2023a). Effect of strain rate on the microstructure evolution and tensile behavior of medium manganese steel. Mater. Lett.330, 133243. 10.1016/j.matlet.2022.133243

  • 60

    MohapatraS.DasK.DasS. (2023b). Significance of intercritical annealing temperature on the impact behavior. Mater. Lett.344, 134418. 10.1016/j.matlet.2023.134418

  • 61

    MohapatraS.PoojariG.DasS.DasK. (2023c). Insights into the dynamic impact behavior of intercritically annealed automotive-grade Fe–7Mn–4Al −0.18C steel. Mater. Sci. Eng. A887, 145769. 10.1016/j.msea.2023.145769

  • 62

    MohapatraS.PalaiD.SatpathyB.DasS.DasK. (2023d). Electrochemical study of intercritically annealed Fe-0.18C-7Mn-4Al steel. Mater. Today Commun.34, 105282. 10.1016/j.mtcomm.2022.105282

  • 63

    MohapatraS.MandalA.PoojariG.DasS.DasK. (2023e). Influence of intercritical annealing temperature on microstructure, microtexture, and tensile behavior of TRIP-assisted medium manganese steel. Materialia28, 101781. 10.1016/j.mtla.2023.101781

  • 64

    MohapatraS.DasK.DasS. (2023f). Study on strain distribution and texture evolution of Fe-0.18C-4Al-7Mn steel under different strain rate conditions. Mater. Lett.354, 135343. 10.1016/j.matlet.2023.135343

  • 65

    MohapatraS.Kumar PradhanS.OhM.-S. (2024a). The impact of annealing temperature and time on the grain distribution and texture evolution of cold-rolled electric-furnace annealed low-carbon steel. Mater. Lett.371, 136955. 10.1016/j.matlet.2024.136955

  • 66

    MohapatraS.PoojariG.SatpathyB.DasS.DasK. (2024b). A comprehensive study on the effect of annealing temperature on the tensile and impact behavior of automotive-grade medium manganese steel (Fe-6.22Mn-0.18C). J. Mater. Eng. Perform.33, 5348–5363. 10.1007/s11665-023-08861-x

  • 67

    MohapatraS.BaekK. C.OhM. S. (2024c). Intercritically annealed medium-manganese steel: insights into microstructural and microtextural evolution, strain distribution, and grain boundary characteristics. Mater. (Basel)17, 2757. 10.3390/ma17112757

  • 68

    MohapatraS.MandalA.DasS.DasK. (2024d). Study on local strain distribution and grain boundary characteristics of tensile-deformed TRIP-assisted medium manganese steel. Mater. Sci. Eng. A894, 146225. 10.1016/j.msea.2024.146225

  • 69

    MohapatraS.SatpathyB.SarkarA.KumarS.AichS. (2025a). Recent advances in medium-manganese steel: a review of key findings, challenges, and future perspectives. J. Mater. Sci.60, 9447–9528. 10.1007/s10853-025-11010-5

  • 70

    MohapatraS.KumarA.KumarS.PoojariG. (2025b). Influence of strain rate on the tensile properties, misorientation distribution, and texture evolution of automotive-grade TRIP-Assisted advanced high-strength steel. Mater. Lett.378, 137612. 10.1016/j.matlet.2024.137612

  • 71

    MohapatraS.SarkarA.KumarS.DalaiR.OhM.-S. (2026a). Impact behavior of automotive grade medium manganese steel: reviews on current progress and challenges. Mater. Sci. Technol.

  • 72

    MohapatraS.KumarS.ArohiA. C.PradhanR.MahapatraB. N. (2026b). Influence of annealing time on microstructure and impact behavior of medium Mn-automotive steel. Mater. Lett.418, 140832. 10.1016/j.matlet.2026.140832

  • 73

    MohapatraS.DasK.DasS.SatpathyB. (2026c). Effect of annealing time on the static and accelerated corrosion behavior of medium manganese steel. J. Mater. Sci.61, 32332–32356. 10.1007/s10853-026-13739-z

  • 74

    Morales-RivasL.ArchieF.ZaeffererS.Benito-AlfonsoM.TsaiS. P.YangJ. R.et al (2018). Crystallographic examination of the interaction between texture evolution, mechanically induced martensitic transformation and twinning in nanostructured bainite. J. Alloys Compd.752:505–519. 10.1016/j.jallcom.2018.04.189

  • 75

    NafisiS.ArafinM. A.CollinsL.SzpunarJ. (2012). Texture and mechanical properties of API X100 steel manufactured under various thermomechanical cycles. Mater. Sci. Eng. A531:2–11. 10.1016/j.msea.2011.09.072

  • 76

    OmaleJ. I.OhaeriE. G.TiamiyuA. A.EskandariM.MostafijurK.SzpunarJ. (2017). Microstructure, texture evolution and mechanical properties of X70 pipeline steel after different thermomechanical treatments. Mater. Sci. Eng. A703:477–485. 10.1016/j.msea.2017.07.086

  • 77

    PanH.ChaofanW.ZhangH.LiX.LiuL.LiJ.et al (2023a). Strain rate sensitivity of low-temperature superplastic cold-rolled medium Mn steel with ultrafine equiaxed dual-phase microstructure. Mater. Sci. Eng. A873, 145025. 10.1016/j.msea.2023.145025

  • 78

    PanH.LiX.ZhangH.LiuL.LiJ.ZhaoY.et al (2023b). Achieving ultra-high elongation of 1401% in a warm-rolled medium Mn lightweight steel with dual-phase lamellar structure. Mater. Sci. Eng. A862, 144493. 10.1016/j.msea.2022.144493

  • 79

    PanH.LiX.ZhangS.ZhouW.WuZ.LiuL. (2023c). Effect of strain rate on the microstructure evolution and superplastic deformation behavior of cold-rolled medium Mn lightweight steel. Mater. Sci. Eng. A879, 145241. 10.1016/j.msea.2023.145241

  • 80

    PatraA. K.KapoorR.MandalS.K.C.H. K.VadlamaniS. S. (2024). Influence of strain rate on the work hardening, strain induced martensite formation, strain partitioning, and variant selection in a medium-Mn steel. Mater. Sci. Eng. A902, 146593. 10.1016/j.msea.2024.146593

  • 81

    PengF.XuY.GuX.WangY.LiuX.LiJ. (2018). The relationships of microstructure-mechanical properties in quenching and partitioning (Q&P) steel accompanied with microalloyed carbide precipitation. Mater. Sci. Eng. A723, 247–258. 10.1016/j.msea.2018.03.061

  • 82

    PierceD. T.JiménezJ. A.BentleyJ.RaabeD.WittigJ. (2015). The influence of stacking fault energy on the microstructural and strain-hardening evolution of Fe-Mn-Al-Si steels during tensile deformation. Acta Mater.100, 178–190. 10.1016/j.actamat.2015.08.030

  • 83

    PoojariG.KumarH.SampreethS.TharianT.MakineniS. K.SinghS. B.et al (2024). Materialia effect of prior cold rolling and aging temperature on PH martensitic stainless steel: evolution of microstructure, micro-texture and austenite stability. Materialia33, 102040. 10.1016/j.mtla.2024.102040

  • 84

    PradhanR.MohapatraS.SunnyM. R.SarkarA. (2024). An investigation on microstructure-texture of E250BR steel plate subjected to post-weld vibration. Proc. Inst. Mech. Eng. Part B J. Eng. Manuf.238, 514–523. 10.1177/09544054231178972

  • 85

    PützR. D.AllamT.WangJ.NowakJ.HaaseC.Sandlöbes-HautS.et al (2021). Control of Electrochemical Corrosion Properties by Influencing Mn Partitioning Through Intercritically Annealing of Medium-Mn Steel, 1–23.

  • 86

    RaabeD. (1997). Texture and microstructure evolution during cold rolling of a strip cast and of a hot rolled austenitic stainless steel. Acta Mater.45, 1137–1151. 10.1016/S1359-6454(96)00222-4

  • 87

    RaabeD.PongeD.DmitrievaO.SanderB. (2009). Nanoprecipitate-hardened 1.5 GPa steels with unexpected high ductility. Scr Mater.60, 1141–1144. 10.1016/j.scriptamat.2009.02.062

  • 88

    RayR. K.JonasJ. J. (1990). Transformation textures in steels. Int. Mater. Rev.35, 1–36. 10.1179/095066090790324046

  • 89

    RazmpooshM. H.MacwanA.BiroE.ZhouY. (2020). Microstructure and dynamic tensile characteristics of dissimilar fiber laser welded advanced high strength steels. Mater. Sci. Eng. A773, 138729. 10.1016/j.msea.2019.138729

  • 90

    RidloF.ZhangB.AkkusC.GulbayO.ChakrabortyA.HuB.et al (2025). Influence of aluminum on microstructure and mechanical properties of air-hardened medium manganese steel. Steel Res. Int.96, 2400869. 10.1002/srin.202400869

  • 91

    SahooB. K.SrivastavaV. C.MahatoB.Ghosh ChowdhuryS. (2021). Microstructure-mechanical property evaluation and deformation mechanism in Al added medium Mn steel processed through intercritical rolling and annealing. Mater. Sci. Eng. A799, 140100. 10.1016/j.msea.2020.140100

  • 92

    SarkarA.SanyalS.BandyopadhyayT. K.MandalS. (2019). Implications of microstructure, Taylor factor distribution and texture on tensile properties in a Ti-added Fe-Mn-Al-Si-C steel. Mater. Sci. Eng. A767, 138402. 10.1016/j.msea.2019.138402

  • 93

    SeoE. J.ChoL.EstrinY.De CoomanB. C. (2016). Microstructure-mechanical properties relationships for quenching and partitioning (Q&P) processed steel. Acta Mater.113, 124–139. 10.1016/j.actamat.2016.04.048

  • 94

    ShaoC.HuiW.ZhangY.ZhaoX.WengY. (2017). Microstructure and mechanical properties of hot-rolled medium-Mn steel containing 3% aluminum. Mater. Sci. Eng. A682, 45–53. 10.1016/j.msea.2016.11.036

  • 95

    SinghA.PatraA. K.AthreyaC. N.SankaranS.SarmaV. S. (2023). Role of Mn content on processing maps, deformation kinetics, microstructure and texture of as-cast medium Mn (6–10 wt% Mn) steels. Mater. Sci. Eng. A884, 145500. 10.1016/j.msea.2023.145500

  • 96

    SoleimaniM.KalhorA.MirzadehH. (2020). Transformation-induced plasticity (TRIP) in advanced steels: a review. Mater. Sci. Eng. A795, 140023. 10.1016/j.msea.2020.140023

  • 97

    SolimanM.PalkowskiH. (2014). Microstructure development and mechanical properties of medium carbon carbide-free bainite steels. Procedia Eng.81, 1306–1311. 10.1016/j.proeng.2014.10.148

  • 98

    SongH.KwonY.SohnS. S.KooM.KimN. J.LeeB. J.et al (2018). Improvement of tensile properties in (austenite+ferrite+κ-carbide) triplex hot-rolled lightweight steels. Mater. Sci. Eng. A730, 177–186. 10.1016/j.msea.2018.06.003

  • 99

    SripushpaK.CheremisinaE.InoueR.IwamaT.UedaS.KamarajA. (2026). Sustainable direct Mn alloying practice to produce medium Mn steel. J. Sustain Metall.12, 1667–1680. 10.1007/s40831-026-01420-3

  • 100

    SteinederK.KrizanD.SchneiderR.BéalC.SommitschC. (2017). On the microstructural characteristics influencing the yielding behavior of ultra-fine grained medium-Mn steels. Acta Mater.139, 39–50. 10.1016/j.actamat.2017.07.056

  • 101

    SuhD. W.KimS. J. (2017). Medium Mn transformation-induced plasticity steels: recent progress and challenges. Scr Mater.126, 63–67. 10.1016/j.scriptamat.2016.07.013

  • 102

    SunB.Kwiatkowski da SilvaA.WuY.MaY.ChenH.ScottC.et al (2022). Physical metallurgy of medium-Mn advanced high-strength steels. Int. Mater. Rev.68, 786–824. 10.1080/09506608.2022.2153220

  • 103

    SuwasS.RayR. K.Satyam SuwasR. K. R. (2014). Crystallographic Texture of Materials.

  • 104

    TirumalasettyG. K.Van HuisM. A.KwakernaakC.SietsmaJ.SloofW.ZandbergenH. (2012). Deformation-induced austenite grain rotation and transformation in TRIP-assisted steel. Acta Mater.60, 1311–1321. 10.1016/j.actamat.2011.11.026

  • 105

    VaranasiR. S.Lipińska-ChwałekM.MayerJ.GaultB.PongeD. (2022). Mechanisms of austenite growth during intercritical annealing in medium manganese steels. Scr Mater.206, 114228. 10.1016/j.scriptamat.2021.114228

  • 106

    VenkatsuryaP. K. C.JiaZ.MisraR. D. K.MulhollandM.ManoharM.HartmannJ.Jr. (2012). Understanding mechanical property anisotropy in high strength niobium-microalloyed linepipe steels. Mater. Sci. Eng. A556:194–210. 10.1016/j.msea.2012.06.078

  • 107

    VenkatsuryaP. K. C.MisraR. D. K.MulhollandM. D.ManoharM.HartmannJ.Jr. (2013). Effect of microstructure on the mechanical properties and texture in high strength 560MPa linepipe steels. Mater. Sci. Eng. A575:6–14. 10.1016/j.msea.2013.03.040

  • 108

    WangM. M.TasanC. C.PongeD.KostkaA.RaabeD. (2014). Smaller is less stable: size effects on twinning vs. transformation of reverted austenite in TRIP-maraging steels. Acta Mater.79, 268–281. 10.1016/j.actamat.2014.07.020

  • 109

    WangX. G.LiuC. H.HeB. B.JiangC.HuangM. (2019). Microscopic strain partitioning in Lüders band of an ultrafine-grained medium Mn steel. Mater. Sci. Eng. A761, 138050. 10.1016/j.msea.2019.138050

  • 110

    WangL.ZhouP.HuY.WangB. (2022). Effect of microstructure and texture on the mechanical properties in high strength pipeline bend. Int. J. Press Vessel Pip.195:104604. 10.1016/j.ijpvp.2021.104604

  • 111

    WangM.LiangX.RenW.TongS.SunX. (2023). Effect of Mn content on the toughness and plasticity of hot-rolled high-carbon medium manganese steel. Mater. (Basel)16, 2299. 10.3390/ma16062299

  • 112

    WrightS. I.FieldD. P. (1998). Recent studies of local texture and its influence on failure. Mater. Sci. Eng. A257:165–170. 10.1016/S0921-5093(98)00835-1

  • 113

    WuZ.JingC.FengY.LiZ.LinT.ZhaoJ.et al (2023). Effect of a new pretreatment-Q&P process on the microstructure and mechanical properties of light-weight Al-containing medium-Mn steels. Mater. Sci. Eng. A862, 144468. 10.1016/j.msea.2022.144468

  • 114

    XiaW.ZhaoX.YueL.ZhangZ. (2020). Microstructural evolution and creep mechanisms in Ni-based single crystal superalloys: a review. J. Alloys Compd.819:152954. 10.1016/j.jallcom.2019.152954

  • 115

    XieC.NakamachiE. (2002). Investigations of the formability of BCC steel sheets by using crystalline plasticity finite element analysis. Mater. Des. - MATER Des.23, 59–68. 10.1016/S0261-3069(01)00043-7

  • 116

    XuL. L.ZhengZ. B.YangH. K.XuZ. b.LongJ.WangS.et al (2025). Adapting medium manganese steels for different wear conditions: insights from aluminum modification. J. Iron Steel Res. Int.32, 3504–3519. 10.1007/s42243-025-01516-2

  • 117

    YadavM. K.KumarD.KumarN.BandyopadhyayT. K. (2023). Hot-rolled Al-added medium Mn steel (Fe-8Mn-2.85Al-1Si-0.2C): microstructural evolution and tensile behavior. Materialia29, 101790. 10.1016/j.mtla.2023.101790

  • 118

    YanS.LiuX.LiangT.ZhaoY. (2018). The effects of the initial microstructure on microstructural evolution, mechanical properties and reversed austenite stability of intercritically annealed Fe-6.1Mn-1.5Si-0.12C steel. Mater. Sci. Eng. A712, 332–340. 10.1016/j.msea.2017.11.118

  • 119

    YanS.LiangT.ChenJ.LiT.LiuX. (2019). A novel Cu-Ni added medium Mn steel: Precipitation of Cu-rich particles and austenite reversed transformation occurring simultaneously during ART annealing. Mater. Sci. Eng. A746, 73–81. 10.1016/j.msea.2019.01.014

  • 120

    YangY. G.MiZ. L.XuM.XiuQ.LiJ.JiangH. T. (2018). Impact of intercritical annealing temperature and strain state on mechanical stability of retained austenite in medium Mn steel. Mater. Sci. Eng. A725, 389–397. 10.1016/j.msea.2018.04.041

  • 121

    YuS.DengY. G. (2025). A review of recent developments in microstructures and mechanical properties of medium manganese steels. J. Mater Eng. Perform.34, 16827–16846. 10.1007/s11665-025-10669-w

  • 122

    ZhangX.MiyamotoG.KaneshitaT.YoshidaY.TojiY.FuruharaT. (2018). Growth mode of austenite during reversion from martensite in Fe-2Mn-1.5Si-0.3C alloy: a transition in kinetics and morphology. Acta Mater.154, 1–13. 10.1016/j.actamat.2018.05.035

  • 123

    ZhangB. G.ZhangX. M.LiuH. T. (2020). Microstructural evolution and mechanical properties of Ni-containing light-weight medium-Mn TRIP steel processed by intercritical annealing. Mater. Sci. Eng. A793, 139289. 10.1016/j.msea.2020.139289

  • 124

    ZhangX.TengR.LiuT.ShiY.LvZ.ZhouQ.et al (2022). Improving strength–ductility synergy in medium Mn steel by combining heterogeneous structure and TRIP effect. Mater. Charact.184, 111661. 10.1016/j.matchar.2021.111661

  • 125

    ZhangH. T.LiH. Y.YanH. L.TangS.BeladiH.HodgsonP.et al (2023). The effect of Ti-Mo additions on microstructural evolution and superplastic deformation behavior of cold–rolled medium Mn steels. Mater. Charact.203, 113051. 10.1016/j.matchar.2023.113051

  • 126

    ZhaoS.SongR.ZhangY.HuoW.CaiC.WangY.et al (2023). Inhibition mechanism of heterogeneous grain structures on plastic instability behavior in 3Mn steel. Mater. Sci. Eng. A874, 145083. 10.1016/j.msea.2023.145083

  • 127

    ZhouN.SongR.LiX.LiJ. (2018). Dependence of austenite stability and deformation behavior on tempering time in an ultrahigh strength medium Mn TRIP steel. Mater. Sci. Eng. A738, 153–162. 10.1016/j.msea.2018.09.098

  • 128

    Zinsaz-borujerdiA.Zarei-hanzakiA.AbediH. R.Karam-AbianM.DingH.HanD.et al (2018). Room temperature mechanical properties and microstructure of a low alloyed TRIP-assisted steel subjected to one-step and two-step quenching and partitioning process. Mater. Sci. Eng. A725, 341–349. 10.1016/j.msea.2018.04.042

  • 129

    ZouY.XuY. B.HuZ. P.ChenS.HanD.MisraR.et al (2017). High strength-toughness combination of a low-carbon medium-manganese steel plate with laminated microstructure and retained austenite. Mater. Sci. Eng. A707, 270–279. 10.1016/j.msea.2017.09.059

  • 130

    ZuoW.YangY.HuY.LiR.ZhangS.WuY.et al (2026). Role of initial microstructures in governing austenite reversion kinetics and morphology in medium manganese steel. J. Mater. Res. Technol.40:1821–1837. 10.1016/j.jmrt.2025.12.265

Summary

Keywords

austenite, intercritical annealing, medium-manganese steel, texture evolution, TRIP effect

Citation

Mohapatra S, Pradhan R, Mahapatra BN and Swain PK (2026) A comprehensive review on development of texture in automotive-grade medium manganese steel. Front. Mater. 13:1954859. doi: 10.3389/fmats.2026.1954859

Received

31 July 2026

Revised

14 September 2026

Accepted

29 September 2026

Published

21 October 2026

Volume

13 - 2026

Edited by

Mattia Franceschi, Spanish National Research Council (CSIC), Spain

Reviewed by

Jessy Michla J. R., Kalasalingam University, India

Harsha B P, PES Institute of Technology and Management, India

Updates

Copyright

*Correspondence: Sudipta Mohapatra,

Disclaimer

All claims expressed in this article are solely those of the authors and do not necessarily represent those of their affiliated organizations, or those of the publisher, the editors and the reviewers. Any product that may be evaluated in this article or claim that may be made by its manufacturer is not guaranteed or endorsed by the publisher.

Outline

Figures

Cite article

Copy to clipboard


Export citation file


Share article

Article metrics