Abstract
This study investigates the profound impact of residual solvents and thermal history on the CO2/CH4 and CO2/N2 separation performance of 6FDA-based polyimide membranes by providing a comprehensive understanding of how solvent-polymer-penetrant interactions dictate macroscopic separation efficiency. Dense 6FDA-DAM membranes were cast using three solvent molecules with varying boiling points (NMP, DMF, and THF) and subjected to distinct annealing protocols (sub-boiling, supra-boiling, and near the glass transition temperature, Tg). Experimental evaluations underscore the persistent nature of solvent entrapment; achieving a completely solvent-free matrix is practically unattainable, as solvent molecules become structurally locked within the polymer chains depending on the evaporation kinetics. These trapped solvents act as plasticizers, expanding fractional free volume and increasing permeability at the expense of selectivity. Conversely, precise thermal treatment near Tg significantly tightens polymer chain packing, effectively doubling CO2/CH4 selectivity, with a considerable drop in CO2 permeability, as the minute amount of remaining trapped solvent begins to act as an anti-plasticizer. To elucidate these macroscopic findings, molecular simulations were performed to capture the coupled effects of the residual solvent and CO2 on rigid (6FDA-DAM) and flexible (6FDA-ODA) polyimide matrices. The computational models emphasize that structural alterations are driven by the combined presence of both CO2 and the trapped solvent, rather than the isolated effect of the solvent. This reveals a direct competition between CO2 and the solvent for preferential sorption sites, primarily nitrogen in the imide group and ether linkages. Furthermore, fractional free volume (FFV) analyses identified a critical transition threshold (1–2 wt% solvent content) where this combined interaction reverses the matrix behavior from synergistic plasticization to anti-plasticization with the decrease of residual solvent content. By detailing the dependence of gas transport properties on both specific solvent selection and thermal treatment, this dual-methodological work establishes a new fundamental perspective for optimizing the fabrication of high-performance polyimide membranes.
1 Introduction
Membrane-based technologies offer a highly attractive alternative to traditional separation processes, particularly in major industrial applications, such as hydrogen recovery, nitrogen production, natural gas sweetening, and vapor recovery (). Beyond their low energy consumption and cost-effectiveness, membranes excel due to their ease of process integration, compact footprint, and byproduct-free operation. Among various polymeric materials, glassy polyimides stand out in membrane technology because of their exceptional thermal, mechanical, and chemical resistance, combined with superior separation performance. In particular, CO2/CH4 separation has gained significant attention; removing CO2 from natural gas is critical not only to meet pipeline quality standards and boost energy content but also to prevent pipeline corrosion. Additionally, efficient CO2/N2 separation plays a vital role in mitigating greenhouse gas emissions through post-combustion carbon capture and subsequent sequestration.
Gas transport through polymeric membranes is governed by an interplay of intrinsic and extrinsic factors. Intrinsically, parameters such as backbone structure, morphology, chain packing, fractional free volume (FFV), and glass transition temperature (Tg) dictate the baseline separation performance. Extrinsically, the membrane fabrication history plays a critical role (; ; ). Among these processing variables, the choice of casting solvent and the subsequent thermal annealing conditions are paramount in shaping the final transport properties (). Residual solvent molecules trapped within the polymer matrix typically act as plasticizers, increasing chain mobility and artificially boosting gas permeability at the expense of selectivity (). Systematic thermal annealing is widely employed to drive off this residual solvent and induce structural relaxation. Interestingly, literature indicates that as the annealing temperature rises and residual solvent drops below a critical threshold, this plasticization effect can transition into an “anti-plasticization” effect, where restricted chain mobility dramatically alters the expected permeability-selectivity trade-off ().
While numerous experimental studies have extensively documented the plasticizing effect of residual solvents on polymer membranes (; ; ; ; ; ; ; ; ), investigation into the counter-phenomenon of anti-plasticization remains remarkably scarce in the literature. Generally, most efforts established that trapped solvent molecules significantly alter membrane morphology, free volume size distribution, and improve gas transport behaviors (; ; ; ; ; ; ; ; ). For instance, Joly et al. () examined 6FDA–mPDA membranes cast with five different solvents, demonstrating that solvents with high molar volumes, such as NMP, leave distinct “imprints” in the polymer matrix that artificially sustain higher permeability. Similarly, Prasad et al. () investigated polyamide-imide (Torlon) membranes cast from NMP, DMAc, and DMF, revealing that CO2 permeability follows the order of NMP > DMAc > DMF whereas the highest CO2/CH4 ideal selectivity is achieved for the membrane prepared from DMAc due to the lower diffusion coefficient of CH4 in the presence of residual DMAc. Backed by 1H NMR spectroscopy and molecular dynamics (MD) simulations, they demonstrated that specific hydrogen-bonding interactions between the polymer backbone and the trapped solvent molecules governed this behavior, i.e., the poor interaction between the residual DMAc with the nonpolar CH4. Additionally, Macchione et al. () highlighted the severe plasticization induced by even trace amounts of solvent; they reported a striking 60 °C reduction in Tg for Hyflon® AD membranes containing just 0.17 wt% residual solvent, which subsequently led to a sharp decline in permselectivity. Beyond plasticization dynamics, the choice of casting solvent fundamentally dictates the initial unrelaxed structure of the membrane (; ; ; ; ; ). Prior works have confirmed this by showing how different solvents dramatically alter membrane surface roughness via Atomic Force Microscopy (AFM) (), shift Tg and FFV values (), and induce significant variations in d-spacing (). In stark contrast to this dominant plasticization narrative, only a limited number of studies have captured the transition to anti-plasticization. A pioneering example is the work by on a novel 6FDA/PMDA-TMMDA polyimide membrane. They revealed that while large amounts of residual solvent act as a plasticizer, the effect completely reverses to anti-plasticization once the solvent content drops below a critical threshold ().
For glassy polymeric membranes, the presence of residual casting solvents is a major issue for long-term stability. Because glassy polymers naturally settle into a denser state over time known as physical aging (; ), any trapped solvent molecules act like molecular lubricants that increase chain mobility and drastically accelerate structural collapse (; ). Initially, these residual molecules can cause anti-plasticization by blocking gas transport pathways, causing a temporary decline in permeability (). Over time, however, the fast-tracked aging leads to an unpredictable decline in gas flux and a sharp rise in selectivity. The situation worsens under exposure to high-pressure condensable gases like CO2. In these conditions, the solvent and the gas combine forces to lead rapid structural relaxation and plasticize the membrane, compromising its operational and mechanical integrity (; ). Therefore, designing reliable membranes for industrial use requires a clear understanding of how trapped solvents, prolonged physical aging, and CO2-induced plasticization interact.
To untangle these interacting phenomena collectively, molecular simulation tools serve as a highly effective alternative. However, computational efforts focused solely on the isolated effects of residual solvent dynamics and their direct impact on polyimide free volume are still remarkably limited (; ; ). Among the few computational attempts, provided molecular-level validation for experimental observations through energetic and radial distribution function (RDF) analyses. They demonstrated that the presence of residual solvent molecules significantly promotes polymer chain flexibility, a classic microscopic indicator of plasticization. Furthermore, they noted that at elevated feed pressures, the influence of the residual solvent on gas sorption diminishes due to competitive sorption mechanisms between gas and solvent molecules (). In another computational study, explored the microstructure and transport behavior of Polymers of Intrinsic Microporosity (PIM-1) as a function of trapped casting solvents. Their simulation results revealed a systematic decrease in FFV and large-size voids following the order of CH3OH > CHCl3 > H2O, showing excellent agreement with experimental positron annihilation lifetime spectroscopy (PALS) data (). adopted a hybrid approach, combining molecular simulations with experimental testing to unravel how DCM and chloroform alter the morphology of Tröger’s base polymers. Backed by thermo-gravimetric analysis (TGA) data showing high chloroform retention, their computational models revealed that chloroform strongly interacts with the polymer matrix, leading to a partial saturation of the sorption sites that ultimately drives down gas permeability ().
To address the gap in the literature, this study is designed around two primary goals that bridge systemic experimental observation with high-pressure molecular modeling. The first goal is to experimentally demonstrate how casting solvent types and precise thermal histories dictate the structural features and subsequent low-pressure CO2/N2 and CO2/CH4 separation performance of polyimide membranes. Unlike traditional literature studies, which predominantly target a single thermal treatment temperature or utilize lone low-temperature drying stages merely to retain residual solvent for plasticization studies, this work implements a strict, highly systematic protocol. Dense 6FDA-DAM membranes were fabricated via the casting–evaporation method using three solvents with distinct boiling points, NMP (204 °C), DMF (153 °C), and THF (67 °C), and systematically annealed across three critical thermal regimes: below the solvent boiling point, above the boiling point, and near the polymer’s Tg. The second goal of this study is to computationally investigate the strength of this residual solvent induced anti-plasticization effect at elevated pressures, where CO2 is known for driving severe polymer plasticization. By carrying out high-pressure molecular simulations, we aimed to explicitly capture how trace amounts of residual solvent and high-pressure CO2 cooperatively or competitively interact within the matrix. Furthermore, to evaluate the role of macromolecular rigidity, these simulations were extended beyond the rigid 6FDA-DAM framework to include the significantly more flexible 6FDA-ODA polyimide matrix, unravelling how chain flexibility influences the competition between penetrants and trapped solvents. Atomistic insights into fractional free volume (FFV), d-spacing, radial distribution functions (RDF), and cohesive energy density (CED) were analyzed to decouple these complex polymer–solvent–penetrant interactions. To the best of our knowledge, this work is the first to offer a detailed molecular-level explanation of how residual solvent thresholds cooperatively drive or suppress CO2-induced plasticization. Ultimately, these findings bridge the gap between processing history and transport performance, offering a predictive blueprint for tailoring next-generation polymeric membranes.
2 Gas transport theory
Gas transport through dense polymeric membranes is typically described by the solution-diffusion mechanism () where the driving force producing movement of a permeant is the gradient in its chemical potential which is related to gradients of pressure, temperature, concentration, and electromotive force. The process of permeation comprises of three steps: sorption of gas molecules on the feed side of the membrane, and then the diffusion across the membrane cross-section via transient gaps in the polymer matrix, and finally desorption from the other surface of the membrane. The separation performance of a membrane is usually defined by its permeability and selectivity. In dense polymeric membranes, this solution-diffusion mechanism is governed on the basis of two distinct but coupled phenomena: thermodynamic solubility and kinetic mobility. On the other hand, strict molecular size-sieving mechanism, where separation relies on well-defined, permanent rigid pore architectures, is predominantly observed in inorganic crystalline materials. Instead, gas transport in these polymeric networks operates fundamentally through the solution-diffusion mechanism.
For a membrane following the solution-diffusion mechanism at isothermal conditions, permeability, P, is defined as the product of diffusivity, D, and solubility or sorption, S, when the downstream pressure is significantly lower than the upstream pressure (Equation 1):
The ideal selectivity for a binary gas feed of A and B (αA/B) is defined as the ratio of pure gas permeabilities (Equation 2):where PA and PB are the permeability coefficients of gases A and B, respectively. By default, the more permeable gas is taken as A, so that selectivity is bigger than 1. The αD and αS represent diffusion selectivity and sorption (solubility) selectivity, respectively. In this study, ideal sorption perm-selectivities of CO2/N2 and CO2/CH4 gas pairs are evaluated by calculating the ratio of the estimated permeability coefficients of the relevant gases.
Valid under isotropic conditions, Fick’s first law governs the diffusion in the absence of bulk flow and is expressed as Equation 3:where J is the diffusive flux, D is the diffusion constant, and C is the concentration of the local gas penetrants. Thus, at any point inside the polymer in Cartesian coordinates, diffusion of gas penetrants in one dimension is given by Equation 4:
Sorption is governed by the inherent condensability of the penetrant molecule and the FFV of the polymer. Over the past three decades, sorption of gas molecules in glassy polymers has been described by the dual-mode sorption model as shown in Equation 5 (; ).
The first term in Equation 5 is described by Henry’s Law relation, and the second term is defined as Langmuir sorption, which is viewed as being due to the uptake into the unrelaxed volume or micro voids present in glassy polymer. Total sorption is the sum of these two effects, where C is the penetrant concentration, p is the pressure, kd is the Henry’s Law constant, b is the hole affinity constant for Langmuir sorption, and C′H is the Langmuir sorption capacity. The ratio of the penetrant concentration to pressure is defined as the sorption coefficient (Equation 6):
In CO2/CH4 and CO2/N2 membrane separation processes, it is known that CO2 acts as a sorption-induced volume swelling agent and/or plasticizer, which hinders the preference of polyimide as a membrane material for gas separation. CO2 induced plasticization is a pressure-dependent phenomenon and occurs when the concentration of CO2 in glassy polymers is high enough to cause swelling in the polymer, i.e., reduce chain alignment and increase inter-segmental mobility and FFV (; ; ; ; ). Due to the loss of size discrimination ability, the permeability of CH4 or N2 increase, leading to a significant decrease in selectivity.
3 Experimental methodology
3.1 Materials
The dianhydride monomer, 4,4'-(Hexafluoroisopropylidene)diphthalic anhydride (6FDA, 99%) were purchased from Sigma-Aldrich, and the diamine monomer, 2,4,6-trimethyl-m-phenylene diamine (DAM, 89%–91%), were purchased from Fluka (see Supplementary Table S1). Prior to the polymerization, the DAM monomer was purified via vacuum sublimation at 85 °C, while the 6FDA monomer was used as received; both monomers were thoroughly dried under vacuum before use. The casting and reaction solvents, including N-Methyl-2-pyrrolidone (NMP, >99.5%, Merck), N,N-Dimethylformamide (DMF, 99.8%, Merck), and tetrahydrofuran (THF, 99.0%, Merck), were used as received without further purification (see Supplementary Table S2). Ortho-dichlorobenzene (o-DCB, ≥98.0%, Merck) was used as the azeotropic dehydration agent during the thermal imidization process, and excess methanol (≥99.9%, Merck) was utilized for the precipitation and washing of the synthesized polyimide. Pure gases used for the permeation measurements (CO2, CH4, and N2) were supplied by Linde Gas with a minimum purity of 99.99%.
3.2 Polymer synthesis
Prior to synthesis, the DAM monomer was purified via vacuum sublimation at 85 °C, while the 6FDA monomer was used as received; both monomers were thoroughly dried before use. The polyimides were synthesized via a conventional two-step solution polymerization technique. In the first step, equimolar amounts of 6FDA and DAM monomers were reacted to form the polyamic acid (PAA) precursor. The reaction was conducted under a continuous nitrogen purge in a three-necked round-bottom flask, maintaining a total monomer concentration of ∼20 wt% in the solvent medium. The solution was continuously stirred at 4 °C for 48 h. This PAA formation step was systematically monitored via Fourier Transform Infrared Spectroscopy (FTIR) between 4000–600 cm-1 until the characteristic precursor peaks (aromatic N–H at 3500 cm-1, –OH of –COOH at 2925 cm-1, and C=O of –COOH at 1680 cm-1) reached a steady state. In the second step, the PAA solution was converted to polyimide through high-temperature thermal imidization at 180 °C in an oil bath, using ortho-dichlorobenzene (o-DCB) as the azeotropic dehydration agent (added in a 1:3 volume ratio relative to NMP). The water generated during the imidization reaction formed a low-boiling azeotrope with o-DCB, which was continuously condensed and separated using a Dean-Stark trap. The excess o-DCB was recycled back into the reactor to maintain a constant solution volume. The progress of the imidization was monitored by tracking the emergence of characteristic polyimide bands in the FTIR spectra, specifically the asymmetric and symmetric C=O stretching at 1780 cm-1 and 1820 cm-1, and the C–N stretching between 1350 cm-1 and 1375 cm-1. Upon completion, the viscous polymer solution was cooled to room temperature and precipitated in excess methanol. The resulting white fibrous precipitate was filtered, washed thoroughly with methanol, and dried under vacuum at 70 °C for 3 days, followed by a final drying stage at 150 °C for 24 h.
3.3 Membrane production
Dense polyimide membranes were fabricated via the solution-casting/solvent-evaporation technique, optimizing the procedure for each specific solvent system. Polymer solutions were prepared at concentrations of 30 wt% for NMP and DMF, and 10 wt% for THF. Prior to casting, a flat glass substrate was thoroughly cleaned and preheated to 100 °C. For the NMP and DMF solutions, the viscous polymer dope was poured onto the heated glass surface and drawn into a uniform thin film using a doctor blade (film applicator) with an initial wet thickness set to 500 μm. These cast films were immediately transferred to a controlled chamber under a continuous nitrogen purge to regulate initial evaporation, followed by further drying in an oven at 80 °C for 2 h to ensure sufficient film solidification. In contrast, due to the high volatility and rapid evaporation rate of THF, the corresponding 10 wt% solution was cast directly into a glass Petri dish and allowed to undergo controlled evaporation under ambient atmospheric conditions. Once completely solidified, all membranes were carefully peeled from their respective glass substrates or Petri dishes. To systematically vary the residual solvent content within the polymer matrices, the self-standing films were subjected to distinct, solvent-specific thermal protocols by being suspended in a vacuum oven, based on both the boiling points of the respective solvents and the Tg of the polyimide, as detailed in Supplementary Figures S1-S3 of the Supplementary Material. Accordingly, the thermal protocols were set at 80, 160, 210, and 385 °C for NMP-cast films; 80, 160, and 385 °C for DMF-cast films; and 30, 80, and 385 °C for THF-cast films. For each thermal treatment step, the membranes were held isothermally at the specified target temperature for specified time, given in Supplementary Figures S1-S3. Subsequently, to consistently lock in the non-equilibrium glassy state and prevent undefined structural variations, the films were cooled to room temperature via natural unassisted cooling within the closed vacuum oven. For clarity and consistency throughout the manuscript, the fabricated membranes are designated using the X/Y-Z nomenclature, where X represents the polyimide type, Y denotes the casting solvent, and Z signifies the final annealing temperature (e.g., 6FDA-DAM/NMP-80).
3.4 Membrane characterization
Standard characterization methods were employed to determine the thermal and structural properties of the membranes. The molecular weight and polydispersity indices of polyimides were evaluated using gel permeation chromatography (GPC, Agilent 1100 Series) in THF on the basis of standard polystyrenes. Thermogravimetric Analysis (TGA) measurements were carried out with a Perkin-Elmer Diamond TG/DTA. About 3 mg of sample was weighed for both film and powder polyimides, and heated from 50 °C to 550 °C at a rate of 20 °C/min. TGA analysis provides information on the amount of moisture and residual solvent in the sample, and were also used as a guide for Differential Scanning Calorimetry (DSC) measurements. DSC analysis was carried out on thin films and powder samples having an average mass of 10 mg using a Perkin-Elmer 4000 Series DSC. To accurately determine the Tg values, a three-stage DSC heating profile was employed under an inert N2 atmosphere at a constant rate of 20 °C/min. The thermal protocol consisted of three consecutive cycles: (i) 30 °C–380 °C, (ii) 30 °C–420 °C, and (iii) 30 °C–450 °C. Tg was calculated based on the third heating by the half-Cp extrapolation method. Wide-angle X-ray diffraction (XRD) patterns of polyimide films were obtained using a PAN analytical X-Pert PRO diffractometer with a CuKα source (λ = 1.54Å). The apparatus scanned over the range of 5°–60°, with a dwell time of 3s and a step size of 0.5°. The d-spacing was calculated from Bragg’s equation, . The average d-spacing is determined from a polynomial curve of the data in the region of the main peak. Polymer film densities at 23 °C were measured with a Ray-Ran density gradient column filled with aqueous zinc chloride-ethanol-water solutions. Each film density was measured at least twice.
While advanced techniques such as Positron Annihilation Lifetime Spectroscopy (PALS) or analytical methods such as NMR spectroscopy or GC-MS offer detailed microstructural and quantitative insights, this study employs TGA, XRD, and density measurements. These techniques were strategically selected due to their simplicity, widespread availability, and proven reliability in capturing the macroscopic bulk structural trends necessary to evaluate the membrane’s thermal history. TGA provides useful information on the overall release of volatile species from the membranes and can therefore indicate the presence of residual solvent; however, the mass loss cannot be assigned exclusively to the casting solvent because other volatile species, including absorbed moisture, may also contribute. Consequently, TGA should be regarded as an indirect assessment of residual solvent content. Similarly, the XRD and density measurements provide information on changes in average chain packing and bulk free-volume characteristics but do not directly resolve the size and distribution of individual free-volume cavities. PALS would provide a more direct characterization of the sub-nanometer free-volume microstructure.
3.5 Gas permeability measurements
Permeability measurements were carried out using the membrane film, which was sandwiched between aluminum tapes and sealed with an epoxy resin to form a mask. The masked membrane was then placed into the permeation cell with an O-ring on both halves and inserted into a pressure-rise permeation apparatus (). The permeation system comprises a permeation cell, upstream and downstream transducers, a data acquisition system, and a gas chromatograph (GC). Permeability measurements were carried out using the masked membrane film, which was placed into the permeation cell with an O-ring on both halves and inserted into a pressure-rise permeation apparatus. After the evacuation of upstream, downstream, and the membrane for 24 h, permeation experiments were conducted at steady state with a linear rate of pressure increase in the downstream volume. On each membrane sample, permeability measurements for each gas were repeated until the slope of the pressure-vs-time plot remained constant. Permeation measurements were carried out at 35 °C and 4 bar upstream pressure. The permeability coefficient of gas i (N2, CO2, or CH4) was calculated using Equation 7.where dp/dt taken as the leak-corrected pressure-rise rate, V is the volume of the downstream, l is the thickness of the membrane, A is the permeation area of the sample, R is the ideal gas constant, T is the temperature at which the measurement was taken, ΔP is the pressure difference between the upstream and the downstream. Specified the conversion factor is used to report the permeability values in Barrer units, as .
4 Molecular modelling
Sorption simulations were carried out using the sorption module of Accelrys® Materials Studio. The simulation procedure applied was the same as that used in our previous study (). Potential parameters of polyimides and solvents with all-atom representation were adapted from the COMPASS force field. The Van der Waals interactions were calculated by pair-wise addition, with the cut-off distance being set to half of the simulation cell length, and the Ewald summation method was used to calculate the electrostatic interactions.
4.1 Model preparation
The molecular models of 6FDA-ODA and 6FDA-DAM repeat units were initially constructed and geometry-optimized as illustrated in Figures 1a,b. The initial structures, including the incorporation of NMP or THF solvent molecules (see Figures 1c,d) at target concentrations ranging between 1–4 wt%, were packed using the Amorphous Cell module of Materials Studio software. These solvent-embedded polymer matrices were then systematically equilibrated through a rigorous series of molecular dynamics (MD) runs, following a well-established protocol from our previous work (). All MD simulations utilized a time step of 1 femtosecond (fs), with the system temperature and pressure regulated via the Berendsen thermostat and barostat, respectively (). Following structural stabilization, key physical and morphological properties, CED, FFV, and flexibility of the diamine-dianhydride linkage, were computed for each matrix. The comprehensive evaluation of these properties was explicitly targeted to elucidate the molecular-level influence of residual solvent type and concentration on the unrelaxed polymer microstructure. Resolving these atomistic alterations is crucial for establishing a direct correlation between the membrane’s processing history and its subsequent gas separation performance.
FIGURE 1
4.2 Calculation of sorption and characteristic properties
The sorption module of the simulation software was used to carry out the sorption simulations in polyimide matrices via the Grand Canonical Monte Carlo (GCMC) ensemble and the Metropolis Algorithm (). Since the plasticization pressure of polyimide membranes was around 10 bar (; ; ), depending on the CO2 concentration, simulations were performed at 35 °C and 10 bar. Coherent with our previous simulation study (), where we have introduced the sorption-relaxation cycles (SRCs) to reproduce the effect of plasticization, we applied these cycles until the sorption coefficients converged. Solvent molecules were randomly deleted in order to obtain respectively 2, 1, and 0 wt% of solvents in polymer matrices from the matrix including 4 wt% of solvent, and again SRCs were repeated for each solvent concentration.
RDF analysis was systematically utilized to elucidate the structural organization of the amorphous matrices and to map the localized penetrant behaviors at the atomistic scale. In gas separation membrane simulations, RDF serves as a powerful diagnostic tool to precisely identify the specific sorption sites of gas molecules within the polymer network. By computing the probability of finding a target atom at a distance r from a reference center relative to the bulk density, RDF profiles (g(r)) unveil localized molecular affinities, where distinct peaks signify strong intermolecular interactions or coordinated packing. In this work, RDF was specifically deployed to identify the primary CO2 sorption sites on the polyimide backbone, focusing on the specific functional groups highlighted in the chemical structures of Figures 1a,b. Furthermore, RDF tracking allowed us to capture the dynamic alterations within these sorption sites in the presence of residual solvent molecules. By analyzing the structural shifts and peak intensity variations in the g(r) profiles, we successfully decoupled how trapped solvent molecules compete for, deform, or partially block these high-affinity sites, directly revealing the microscopic mechanism behind the solvent-induced changes in CO2 sorption capacity.
The torsional distribution of the dihedral angles (C–N–C–C) along the central dianhydride–diamine linkage was evaluated to monitor the intrinsic macromolecular rigidity of the polymer chain backbones. To further quantify linkage flexibility, the standard deviation of the dihedral angle distribution (σ|φ|) was calculated based on the absolute angular deviations.
The Cohesive Energy Density (CED) serves as a direct indicator of the intermolecular force strengths pinning the polyimide chains within their nearest-neighbor coordination spheres. For a single-chain polymer framework subjected to high penetrant loadings, the CED is explicitly calculated by decoupling the periodic effects as follows Equation 8:where EPBC and Enon-PBC represent the non-bonded potential energies of the polymer matrix evaluated with and without periodic boundary conditions, respectively, and V denotes the equilibrium volume of the simulation cell. Operationally, EPBC was computed utilizing a real-space cut-off distance set to half of the simulation box size, whereas a wider 100 Å cut-off was implemented for Enon-PBC to comprehensively capture all long-range non-bonded interactions across the unraveled matrix. Highly compact, tightly packed matrices typically manifest elevated CED values, which run inversely to FFV and penetrant diffusivity profiles.
FFV determines the structural openness of the glassy polyimide architecture, which serves as a prime thermodynamic lever governing penetrant solubility. FFV values of the model matrices were estimated using the following geometric relation (Equation 6):where Vw is the localized van der Waals volume of the polyimide chains. Rather than relying on semi-empirical group contribution frameworks such as the Bondi method, Vw was computed directly using the Atom Volumes & Surfaces tool with a high-resolution grid spacing. To capture the precise extent of CO2-induced swelling and plasticization trends, the percentage increase in FFV post-sorption (FFV%) was tracked. This parameter tracks how the matrix expands to accommodate dense high-pressure penetrants and trace solvent thresholds, providing a clear molecular understanding of the competitive plasticization–anti-plasticization transition.
5 Results and discussion
5.1 Experimental characteristic properties of polymers
The synthesis of the 6FDA-DAM polyimide was successfully executed via a two-step, one-pot solution imidization protocol. The progressive conversion from the intermediate polyamic acid (PAA) precursor to the fully cyclized, ring-closed polyimide network was systematically monitored via FTIR spectroscopy, as illustrated in Supplementary Figure S4. In the PAA spectrum (Supplementary Figure S4a), characteristic amic acid absorption bands are clearly visible, featuring a distinct aromatic NH–C stretching peak at 3488 cm-1, an O–H stretching vibration associated with the carboxylic acid (–COOH) groups at 2924 cm-1, and a pronounced carboxylic carbonyl (C=O) stretching band localized at 1669 cm-1. Following the successful completion of the thermal imidization step and subsequent exhaustive drying of the resulting powder samples, a structural reorganization is confirmed (Supplementary Figure S4b). Specifically, the final polyimide structure exhibits intense asymmetric and symmetric C=O stretching vibrations at 1788 cm-1 and 1728 cm-1, respectively, complemented by a sharp characteristic C–N linkage stretching mode at 1358 cm-1. This absolute spectral transformation serves as evidence of full chemical conversion and high imidization efficiency without detectable ring-opening side defects.
Beyond structural confirmation, the macromolecular weight distribution of the synthesized polyimides obtained through polymerization step was evaluated via GPC. The resulting weight-average molecular weights (Mw) along with the corresponding polydispersity indices (PDI), Tg, and d-spacing values are systematically summarized in Table 1.
TABLE 1
| Polymer batch | Mw (g/mol) | PDI | Tg ( °C) | d-spacing (Å) |
|---|---|---|---|---|
| PI-1 | 60,000 | 1.6 | 385 | 5.60 |
| PI-2 | 90,000 | 1.9 | 392 | 5.69 |
Characteristic properties of polyimide synthesized in two batches.
Using the polyimide fabrication process described in the previous section, two batches of polyimides, designated as PI-1 and PI-2, were synthesized with molecular weights of 60,000 g/mol and 90,000 g/mol, respectively, successfully satisfying the rigorous mechanical and structural thresholds required for high-quality membrane casting. The PDI of the synthesized polyimides fell tightly within a narrow range of 1–2. Achieving a PDI close to the ideal value of 1 is highly critical, as a narrow molecular weight distribution ensures uniform chain lengths throughout the polymer matrix. On the other hand, DSC analysis revealed high Tg of 385 °C and 392 °C for PI-1 and PI-2, respectively. These elevated Tg values are directly governed by the structural features of the DAM diamine moiety. The bulky, space-filling methyl (–CH3) substituents decorated along the phenyl rings of the DAM monomer exert severe steric hindrance, hindering localized sub-segmental chain rotations along the polymer backbone and successfully imparting high macroscopic thermal and structural stability to the 6FDA-DAM network. In the subsequent membrane fabrication stage, the NMP- and DMF-cast membranes were prepared from the PI-1 batch, whereas the THF-cast membranes were produced from the PI-2 batch, and the corresponding results are presented accordingly.
5.2 Experimental characteristic properties of membranes
To establish a clear correlation between the membrane fabrication history and the resulting gas separation performance, a quantitative assessment of the thermal stability and residual solvent content within the polyimide matrices is essential. Thermal gravimetric analysis (TGA) serves as a vital diagnostic tool in this regard, as it tracks the weight loss profile of the membranes to reveal not only the precise amount of trapped solvent molecules but also the structural relaxation induced by different thermal protocols. Since the presence of residual solvents fundamentally alters the FFV and polymer chain mobility, understanding the volatilization thresholds and the ultimate thermal decomposition behavior is a prerequisite for interpreting transport mechanisms. Therefore, the thermal stability profiles observed from TGA for the solvent-cast 6FDA-DAM membranes are presented in Figure 2, with their corresponding cumulative mass loss percentages across defined temperature intervals compiled in Table 2. As a general trend, membranes annealed at lower temperatures (e.g., 80 °C or 30 °C) exhibit significantly higher mass losses below 300 °C compared to those subjected to high-temperature thermal treatment. This directly confirms that when the processing temperature is maintained well below the boiling point of the casting solvent, a substantial fraction of the solvent becomes trapped within the unrelaxed polymer matrix. For instance, when comparing membranes cast from different solvents but treated at the same temperature (80 °C), 6FDA-DAM/NMP-80 displays a cumulative mass loss of 10.40% at 300 °C, which is markedly higher than that of 6FDA-DAM/DMF-80 (7.50%) and 6FDA-DAM/THF-80 (2.00%). This distinction is directly governed by the boiling points of the solvents; NMP (204 °C) requires considerably higher thermal energy to desorb from the glassy polyimide membrane compared to the highly volatile THF (67 °C).
FIGURE 2
TABLE 2
| Membranes | Cumulative Mass loss % (50 °C–550 °C) | |||||||||
|---|---|---|---|---|---|---|---|---|---|---|
| 100 | 150 | 204 | 250 | 300 | 350 | 385 | 450 | 500 | 550 | |
| 6FDA-DAM/NMP-80 | 0.182 | 1.66 | 5.53 | 8.36 | 10.4 | 11.4 | 11.6 | 11.9 | 13.5 | 21.1 |
| 6FDA-DAM/NMP-160 | 0.054 | 0.104 | 0.216 | 0.499 | 0.868 | 0.957 | 1.30 | 1.77 | 3.34 | 13.9 |
| 6FDA-DAM/NMP-210 | 0.246 | 0.682 | 1.39 | 1.91 | 2.36 | 2.69 | 2.92 | 3.58 | 5.31 | 13.7 |
| 6FDA-DAM/NMP-385 | 0.538 | 0.930 | 1.25 | 1.76 | 2.28 | 2.67 | 2.85 | 3.74 | 6.44 | 15.1 |
| 6FDA-DAM (powder) | 0.227 | 0.905 | 3.31 | 4.96 | 5.18 | 5.31 | 5.48 | 5.89 | 7.63 | 15.8 |
| | 100 | 153 | 200 | 250 | 300 | 350 | 385 | 450 | 500 | 550 |
| 6FDA-DAM/DMF-80 | 0.166 | 1.42 | 4.05 | 6.17 | 7.50 | 8.15 | 8.46 | 8.98 | 10.9 | 18.7 |
| 6FDA-DAM/DMF-160 | 0.175 | 0.632 | 1.46 | 2.16 | 2.37 | 2.74 | 3.11 | 4.12 | 6.65 | 15.7 |
| 6FDA-DAM/DMF-385 | 0.105 | 0.271 | 0.398 | 0.405 | 0.520 | 0.604 | 0.917 | 4.01 | 9.02 | 17.9 |
| 6FDA-DAM (powder) | 0.227 | 0.905 | 3.31 | 4.96 | 5.18 | 5.31 | 5.48 | 5.89 | 7.63 | 15.8 |
| | 67 | 100 | 150 | 200 | 250 | 300 | 350 | 392 | 450 | 500 |
| 6FDA-DAM/THF-30 | 0.077 | 0.380 | 1.88 | 4.49 | 7.16 | 8.43 | 9.18 | 9.64 | 10.4 | 12.1 |
| 6FDA-DAM/THF-80 | 0.009 | 0.096 | 0.266 | 0.779 | 2.00 | 3.10 | 3.92 | 4.44 | 5.13 | 6.79 |
| 6FDA-DAM/THF-385 | 0.037 | 0.192 | 0.352 | 0.378 | 0.426 | 0.497 | 0.669 | 1.00 | 3.56 | 8.25 |
| 6FDA-DAM (powder) | ― | 0.104 | 0.322 | 1.12 | 1.94 | 2.25 | 2.32 | 2.45 | 2.75 | 4.47 |
Measured mass loss amounts at specific temperatures derived from TGA for 6FDA-DAM membranes cast using three different solvents.
Boiling temperatures of NMP, DMF, and THF, are 204, 153, and 67 °C, respectively. NMP- and DMF-based membrane series were prepared from the polymer powder having Tg of 385 °C, whereas polymer powder with Tg of 392 °C was used in the THF-based membrane series. At these specific values, the weight loss was also recorded.
A closer look at the high-temperature annealed samples (indicated by the green curves at 385 °C in Figure 2) reveals a distinct thermal stabilization effect. Contrary to sub-boiling treatments, where gradual weight loss occurs continuously due to solvent evaporation, membranes annealed at 385 °C maintain an almost flat baseline up to approximately 450 °C. This indicates that high-temperature annealing effectively cleanses the free volume of residual solvent molecules. Consequently, the absence of solvent-induced plasticization enhances the overall thermal resistance of the polymer network, shifting the onset of main-chain polymer decomposition to higher temperatures. Among the membranes annealed near the polymer Tg (385 °C), the NMP-cast membrane exhibits a slightly delayed thermal decomposition compared to the DMF and THF membranes. This behavior likely originates from the initial film-formation phase. The significantly slower evaporation kinetics of NMP may provide the polymer chains with an extended window to naturally relax and adopt a denser packing conformation before vitrification. This initially compact morphology appears to influence the structural relaxation pathways during high-temperature annealing, ultimately yielding a matrix that requires slightly more thermal energy to degrade. However, given the relatively minor shift in decomposition temperature, this interpretation serves as a qualitative indicator of solvent-dependent chain packing rather than definitive structural proof.
The most remarkable behavior was observed within the NMP-based membrane series. Interestingly, as detailed in Table 2, 6FDA-DAM/NMP-160 exhibits an exceptionally low cumulative mass loss of only 0.868% at 300 °C, which is significantly lower than that of 6FDA-DAM/NMP-80 (10.40%), but also unexpectedly lower than the higher-temperature treated counterparts, 6FDA-DAM/NMP-210 (2.362%) and 6FDA-DAM/NMP-385 (2.276%). This counterintuitive trend suggests that annealing at a sub-boiling temperature (160 °C) provides an optimal kinetic window for solvent desorption. At this temperature, steady solvent removal may delay immediate structural collapse, instead inducing a temporary structural expansion as evidenced by the remarkably high d-spacing of 6.13 Å (Table 3). This expanded free volume network temporarily maintains open diffusion pathways for efficient solvent evacuation. In contrast, applying thermal energy near or above the boiling point (210 °C and 385 °C) triggers rapid flash evaporation, leading to premature structural chain compaction, which is directly corroborated by the sudden drop in d-spacing (e.g., down to 5.99 Å for NMP-210). This sudden compaction may slam the diffusion pathways shut, inadvertently encapsulating the remaining trace solvent molecules within isolated voids.
TABLE 3
| Membranes | Tg ( °C) | Density (g/cm3) | d-spacing (Å) |
|---|---|---|---|
| 6FDA-DAM/NMP-80 | 383.7 | 1.446 ± 0.005 | 5.61 |
| 6FDA-DAM/NMP-160 | 385.1 | 1.451 ± 0.017 | 6.13 |
| 6FDA-DAM/NMP-210 | 389.0 | 1.445 ± 0.006 | 5.99 |
| 6FDA-DAM/NMP-385 | ― | 1.529 ± 0.050 | 5.98 |
| 6FDA-DAM (powder) | 385.0 | ― | 5.60 |
| 6FDA-DAM/DMF-80 | 384.4 | 1.444 ± 0.012 | 5.79 |
| 6FDA-DAM/DMF-160 | 380.4 | 1.437 ± 0.008 | 6.16 |
| 6FDA-DAM/DMF-385 | ― | 1.485 ± 0.077 | 5.74 |
| 6FDA-DAM (powder) | 385.0 | ― | 5.60 |
| 6FDA-DAM/THF-30 | 383.3 | 1.503 ± 0.074 | 5.70 |
| 6FDA-DAM/THF-80 | 385.2 | 1.462 ± 0.027 | 5.60 |
| 6FDA-DAM/THF-385 | ― | 1.477 ± 0.036 | 6.17 |
| 6FDA-DAM (powder) | 392.0 | ― | 5.69 |
Experimental characteristic properties of solvent-based membranes.
Considering the d-spacing values reported in Table 3, typically, a linear relationship is expected between the thermal history and chain packing; however, membranes treated near or slightly below their solvent’s boiling points, such as 6FDA-DAM/NMP-160, 6FDA-DAM/DMF-160, and 6FDA-DAM/THF-80, deviate from this trend by displaying anomalously high d-spacing values. This supporting evidence validates the hypothesis that localized solvent-polymer interactions at these specific thermal windows induce a structural expansion that expands the interchain distance. While the trapped solvent concentration in DMF and THF series was too low to be clearly distinguished solely by TGA weight loss, their explicit deviations from the d-spacing trend reinforce the universal impact of processing history (sub-boiling treatment) on the sub-microscopic architecture of polyimide membranes. It should be emphasized that such localized sub-microscopic variations do not necessarily translate to proportional macroscopic changes. Since bulk density and XRD d-spacing probe entirely different structural length scales during solvent desorption, we avoid from drawing direct quantitative correlations between them.
Generally, the Tg values exhibit a linear relationship with the residual solvent content, where a decrease in trapped solvent minimizes plasticization and leads to a higher Tg (as observed in the NMP and THF series). However, 6FDA-DAM/DMF-160 deviates from this trend, showing a noticeably lower Tg (380.4 °C) than 6FDA-DAM/DMF-80 (384.4 °C) despite containing less solvent. While such localized anomalies could theoretically be associated with early structural shifts during the transition to anti-plasticization, Tg alone cannot be used to definitively explain this mechanism across all systems. This is particularly evident given the absence of this trend in the THF series at 80 °C, coupled with the inability to reliably resolve the Tg for the fully annealed key samples at 385 °C. On the other hand, it is particularly compelling to contrast the high thermomechanical stability of the 6FDA-DAM network with other glassy polymers in the literature. For instance, Macchione et al. () reported a striking 60 °C reduction in Tg for perfluorinated Hyflon® AD membranes containing merely 0.17 wt% residual solvent. In stark contrast, our 6FDA-DAM membranes exhibit a marginal Tg shift of only ∼1 °C (Table 3) despite retaining over ∼10 wt% residual solvent (e.g., 6FDA-DAM/NMP-80). This discrepancy results directly from the fundamental differences in macromolecular structures. Unlike flexible aliphatic or perfluorinated backbones, 6FDA-DAM is a completely aromatic polyimide characterized by extreme backbone rigidity. The severe steric hindrance imposed by the bulky -C(CF3)2- linkages and the trimethyl-substituted DAM phenyl rings drastically restricts large-scale segmental mobility. Consequently, the highly constrained aromatic network physically resists solvent-induced segmental relaxation, requiring very high thermal energy to trigger the glass transition regardless of the substantial amount of trapped solvent bulk.
5.3 Gas separation properties of membranes
The gas separation performance measured at 35 °C and 4 bar of the fabricated 6FDA-DAM membranes was evaluated to understand the direct consequences of processing history and residual solvent profiles on productivity and efficiency. The ideal selectivity versus CO2 permeability trade-off curves for NMP, DMF, and THF-cast membrane series are illustrated in Figures 3a–c, respectively (see Supplementary Table S3 for raw data). It should be noted that all permeation measurements were performed at least in duplicate on replicate films to ensure reproducibility. The results demonstrated high consistency, successfully excluding the presence of macroscopic defects (e.g., pinholes), which allows us to attribute specific permeation anomalies to intrinsic matrix plasticization rather than film failure.
FIGURE 3
While the NMP and DMF series broadly follow a general upper-left migration trend towards higher selectivity and lower permeability upon progressive thermal annealing, the highly volatile THF series exhibits a specific deviation. Notably, the initial thermal step for the THF-cast film (from 30 °C to 80 °C) causes the CO2/CH4 selectivity to fall from 28.3 to 21.9, disrupting the general trend before recovering at higher annealing temperatures. This progressive loss in CO2 permeability for NMP and DMF series, accompanied by a simultaneous increase in ideal selectivity, is heavily dictated by the sub-microscopic structural relaxation of the polymer matrix. As higher thermal energy is supplied, the continuous desorption of trapped solvent molecules eliminates the solvent-induced plasticization effect, forcing the glassy polyimide chains to contract, restrict their segmental mobility, and undergo a tighter chain packing ().
Closer inspection of the transition states reveals compelling evidence for the reversal from a plasticized state to an anti-plasticization regime, echoing the unique thermal trends observed in our TGA data (see Table 2). When evaluating the intermediate thermal protocols, specifically the shift from the initial low-temperature states (open symbols) to 6FDA-DAM/NMP-160, 6FDA-DAM/DMF-160, and 6FDA-DAM/THF-80 (tracked by the black dashed arrows), for all three solvent systems, the membranes experience a localized increase in CO2 permeability during this first thermal step. For instance, in the NMP-cast series, the permeability rises from 236 Barrer (open symbol, 6FDA-DAM/NMP-80) to nearly 387 Barrer (filled symbol, 6FDA-DAM/NMP-160), a trend tightly echoed by the DMF and THF series as well. The counter-intuitive behavior observed at intermediate annealing temperatures may reflect a competition between residual-solvent removal and polymer-chain relaxation, rather than a universal solvent-desorption-induced expansion mechanism. The relative importance of these processes is strongly dependent on the casting solvent and the thermal treatment. For the THF-cast membranes, heating from 30 °C to 80 °C crosses the relatively low boiling point of THF (∼67 °C), favoring rapid solvent removal. Following this removal, chain relaxation and local densification may become dominant, consistent with the slight decrease in the XRD-derived d-spacing from 5.70 to 5.60 Å. In contrast, DMF and NMP have substantially higher boiling points (∼153 and ∼204 °C, respectively), and their removal from the glassy polymer matrix may occur over broader thermal windows. For NMP in particular, annealing at 160 °C occurs below its normal boiling point, such that residual-solvent removal is more appropriately considered a diffusion- and desorption-controlled process coupled with polymer-chain rearrangement. The increases in d-spacing observed for the DMF- and NMP-based membranes may therefore reflect differences in average chain packing generated by this coupled solvent-removal/relaxation process. Nevertheless, because the XRD-derived d-spacing represents an average structural parameter rather than the dimensions of individual free-volume cavities, these changes should be regarded as being consistent with solvent-dependent structural rearrangement rather than as direct evidence of free-volume expansion.
Crucially, a holistic comparison of the three solvent systems unveils a compelling performance convergence at the final thermal stage (385 °C). While the membranes exhibit highly divergent, solvent-dependent permeability and selectivity paths at lower and intermediate temperatures, reflecting a strong “solvent memory” effect, their transport properties converge into a nearly identical regime upon fully annealing near the polymer’s Tg. This demonstrates that high-temperature thermal treatment acts as a morphological reset, successfully erasing the processing history induced by the casting solvents.
Intriguingly, this solvent-driven structural compaction exerts distinct impacts on different gas pairs, which can be elucidated through a molecular size-sieving mechanism. As tracked by the continuous arrows leading to the final high-temperature states (385 °C), the CO2/N2 ideal selectivity exhibits only a marginal upward shift across the thermal steps. In stark contrast, the CO2/CH4 selectivity undergoes a dramatic surge, at least doubling when comparing the fully annealed membranes (385 °C) with their initial low-temperature baselines (open symbols). This behavior is directly governed by the structural dimensions and kinetic diameters of the target gases (CO2: 3.30 Å, N2: 3.64 Å, and CH4: 3.80 Å). The high-temperature annealing at 385 °C systematically collapses the larger free volume paths. Because the size exclusion threshold of the newly relaxed 6FDA-DAM network falls precisely between the kinetic diameters of N2 and CH4, the diffusion of the bulkier CH4 molecules is severely obstructed. In contrast, the smaller N2 and CO2 molecules experience less spatial hindrance. These findings conclusively demonstrate that post-casting thermal history, by tuning the threshold concentration of the residual solvent, serves as a powerful lever to alter the sub-nanometer free volume architecture and unlock superior size-sieving capabilities. However, a notable anomaly is observed for just one case, for the heavily plasticized 6FDA-DAM/NMP-80 membrane, where the permeability of larger CH4 molecules slightly exceeds that of smaller N2 (31.2 > 29.6 Barrer). Because replicate measurements ruled out macroscopic film defects, this inversion is attributed to solvent-induced plasticization. The high retention of NMP dilates the matrix, limiting its size-sieving capability.
To compare the performance of 6FDA-DAM membrane with the literature, we tabulated its single-gas permeation data such as CO2, CH4, and N2 permeability and CO2/CH4 and CO2/N2 selectivity values in Supplementary Table S4. Reported CO2 permeabilities for 6FDA-DAM membranes vary in a broad range, typically from approximately 358–1200 Barrer. The highest permeability observed in our study (387 Barrer for 6FDA-DAM/NMP-160) aligns well with the lower bound of this established spectrum. Moreover, following our near-Tg annealing protocol, the CO2 permeability drops by one to two decades, reaching 17–67 Barrer (Figure 3). This deviation underscores the significant impact of thermal history, which governs both physical relaxation and chemical network modifications. Beyond the physical macro-structural chain collapse induced by the extreme thermal energy, heating such polyimides to 385 °C can trigger thermo-oxidative crosslinking of the methyl (-CH3) groups present on the DAM monomer (; ). This chemical rigidification acts synergistically with the physical volumetric compaction to irreversibly restrict segmental mobility and reduce the intrinsic free volume. This dual mechanism completely overrides the typically high-free-volume nature of the bulky 6FDA and DAM moieties, converting the conventionally high-permeability polyimide into an ultra-tight molecular sieve. This suggests that aggressive post-casting thermal protocols can fundamentally rewrite the expected transport properties of rigid glassy polymers.
On top of these, drawing a direct, straightforward quantitative comparison across different studies is inherently challenging. The available literature includes a wide range of processing variables, such as casting solvent type, precise thermal history (temperature and duration), polymer molecular weight, and trace impurities, that are highly variable and sometimes not reported. For instance, previous studies demonstrate that utilizing the exact same casting solvent (THF) and thermal treatment (180 °C for 24 h) can still yield a three-fold difference in CO2 permeability (e.g., from ∼390 to 1200 Barrer ()) simply due to variations in the molecular weight of the synthesized polymer. Additionally, permeability values shift dramatically depending on the specific casting solvent used (such as THF, NMP, or DMAc) and the drying or annealing protocols applied, which range from room temperature up to 270 °C. Each specific combination essentially locks the polymer chains into a completely different state of fractional free volume. This extreme sensitivity illustrates that even minor deviations in these processing parameters can lead to great changes in membrane performance. Viewed within this context, the significant permeability variations observed in our study, driven specifically by solvent evaporation kinetics and thermal annealing, are physically consistent and underscore the profound impact of processing history on rigid glassy polyimides.
5.4 Simulated characteristic properties of polyimide matrices
To complement our experimental observations and unveil the underlying microscopic mechanisms, molecular simulations were carried out at elevated pressures, focusing specifically on NMP and THF as the representative solvent systems. Crucially, it must be emphasized that this computational framework does not aim to establish a direct, quantitative one-to-one mapping between the exact weight percentages embedded in the simulation cells and the experimentally measured residual solvent contents remaining after distinct annealing protocols. To the best of our knowledge, the literature currently lacks standardized protocols for isolating and reporting the absolute thermodynamic mass fractions of trapped solvents immediately post-casting. Therefore, cross-validations between our experimental and computational datasets should be evaluated with care, focusing strictly on the qualitative and quantitative structural trends driven by the variations in residual solvent content.
While the experimental gas transport tests were performed at low-pressure regimes (4 bar), these computational models specifically investigate the high-pressure behavior (10 bar), where CO2 is historically known to induce severe sorption-induced swelling and plasticization. This framework allows us to systematically decouple the competitive or cooperative interactions between high-pressure CO2 penetration and trace amounts of residual solvents (0–4 wt%). Furthermore, to evaluate the decisive role of macromolecular architecture, the computational screening was extended from the experimentally synthesized rigid 6FDA-DAM network to a significantly more flexible 6FDA-ODA polyimide matrix. Therefore, we aimed to investigate how chain flexibility dictates the fine line between solvent-induced anti-plasticization and penetrant-driven plasticization. The computed sub-microscopic structural properties of the 6FDA-DAM and 6FDA-ODA polyimide matrices across varying solvent concentrations are summarized in Table 4.
TABLE 4
| Membranes | Density (g/cm3) | FFV (initial) | FFV (Final) | % increase | CED (MCal/m3) |
|---|---|---|---|---|---|
| 6FDA-DAM/NMP-0% | 1.254 | 0.263 | 0.314 | 19.4 | 49 |
| 6FDA-DAM/NMP-1% | 1.254 | 0.260 | 0.305 | 17.3 | 50 |
| 6FDA-DAM/NMP-2% | 1.253 | 0.258 | 0.297 | 15.1 | 52 |
| 6FDA-DAM/NMP-4% | 1.267 | 0.246 | 0.297 | 20.7 | 53 |
| 6FDA-DAM/THF-0% | 1.255 | 0.263 | 0.290 | 10.3 | 54 |
| 6FDA-DAM/THF-1% | 1.269 | 0.251 | 0.278 | 10.8 | 58 |
| 6FDA-DAM/THF-2% | 1.265 | 0.251 | 0.278 | 10.8 | 59 |
| 6FDA-DAM/THF-4% | 1.251 | 0.252 | 0.295 | 17.1 | 67 |
| 6FDA-ODA/NMP-0% | 1.332 | 0.230 | 0.271 | 17.8 | 64 |
| 6FDA-ODA/NMP-1% | 1.344 | 0.223 | 0.238 | 6.73 | 65 |
| 6FDA-ODA/NMP-2% | 1.351 | 0.214 | 0.242 | 13.1 | 67 |
| 6FDA-ODA/NMP-4% | 1.360 | 0.203 | 0.234 | 15.3 | 76 |
| 6FDA-ODA/THF-0% | 1.316 | 0.239 | 0.275 | 15.1 | 63 |
| 6FDA-ODA/THF-1% | 1.332 | 0.227 | 0.279 | 22.9 | 66 |
| 6FDA-ODA/THF-2% | 1.339 | 0.219 | 0.279 | 27.4 | 69 |
| 6FDA-ODA/THF-4% | 1.361 | 0.200 | 0.272 | 36.0 | 85 |
Simulated characteristic properties of solvent-based membranes.
The Cohesive Energy Density (CED) was initially calculated to quantify the magnitude of intermolecular forces required to separate the polymer chains from their nearest neighbors within the matrix. When comparing the solvent-embedded matrices in Table 4, the THF-containing polyimides consistently display higher CED values than their NMP-containing counterparts, indicating a more closely packed and structurally cohesive unrelaxed network. For instance, at a 4 wt% solvent loading, 6FDA-DAM/THF reaches a CED of 67 MCal/m3 compared to the 53 MCal/m3 recorded for 6FDA-DAM/NMP. A similar and even more pronounced jump is witnessed in the flexible matrix, where 6FDA-ODA/THF-4% hits a high CED value of 85 MCal/m3 against the 76 MCal/m3 of the NMP equivalent. This variation suggests that the highly volatile THF solvent exerts a more drastic initial constraint on the structural strength of the matrix; consequently, its subsequent removal triggers a sharper shift in cohesive energy compared to NMP. Crucially, these CED profiles reflect the cooperative impact of both the trapped solvent molecules and the dissolved high-pressure CO2 penetrants rather than the solvent alone. This computational insight directly provides our experimental processing observations. Because of the high volatility and rapid evaporation rate of THF, the polymer chains are abruptly locked into a highly unrelaxed, kinetically trapped state during the casting stage. This rapid solidification prevents proper macromolecular relaxation, manifests macroscopically as a distinct structural rigidity, and explains why the subsequent thermal removal of THF induces a significantly more abrupt transformation in the membrane’s physical architecture compared to the more gradual desorption kinetics of the high-boiling NMP series.
This cohesive tightening is strongly reflected in the initial FFV shifts before solvent incorporation. Upon introducing 4 wt% solvent, the baseline FFV of the rigid 6FDA-DAM matrix decreases by 6.9% (from 0.263 at 0% to 0.246 at 4% for NMP) and 4.4% (from 0.263 to 0.252 for THF). In stark contrast, the flexible 6FDA-ODA matrix experiences much more massive structural compressions, with initial FFV reductions reaching 13.3% for NMP (0.230 down to 0.203) and a striking 19.5% for THF (0.239 down to 0.200). This substantial volume collapse in the flexible matrix is mirrored by a corresponding densification, where the density of 6FDA-ODA/THF jumps sharply from 1.316 g/cm3 to 1.361 g/cm3, underscoring how unconstrained polymer chains can easily rearrange to accommodate solvent molecules within their free volume voids. However, it is crucial to highlight the mechanistic distinction between the computational density trends and the macroscopic experimental densification. In the molecular modeling protocol, the unrelaxed matrix is initially constructed with 4 wt% solvent. When solvent molecules are computationally deleted to simulate lower contents (0–2 wt%) at 35 °C, the glassy polyimide chains lack sufficient thermal mobility to completely collapse into the newly vacated free volume. Consequently, the loss of solvent mass exceeds the corresponding volumetric shrinkage, leading to a natural decrease in computational density (Table 4). However, the experimental density follows a completely different trajectory governed by its thermal history. The removal of entrapped solvent molecules via high-temperature annealing (385 °C) provides the thermal energy required to overcome kinetic barriers. This triggers a massive macro-structural relaxation and tighter chain packing. This volumetric compaction more than compensates for the slight loss in residual solvent mass, leading to a systematic increase in the experimental density values (by ∼8% for NMP, Table 3). This behavior suggests that densification observed at high-temperature is primarily associated with pronounced structural relaxation and chain packing, rather than solely with solvent evacuation, which dominates the changes observed at lower annealing temperatures.
To map the extent of CO2-induced swelling, the correlation between residual solvent concentration, the percentage of FFV increase after sorption, and polymer backbone flexibility is illustrated in Figure 4, with exact values summarized in Table 4. The percentage increase in FFV serves as a direct indicator of plasticization severity. Intriguingly, the resulting curves display a distinct minimum, providing explicit molecular evidence of a fierce competition between CO2 and the residual solvent. At low solvent thresholds, the anti-plasticization effect dominates; the trapped solvent molecules efficiently occupy and stiffen the local free volume paths, leading to a visible drop in the CO2-induced FFV increase. However, beyond a critical threshold, the combined plasticizing natures of both the presence of residual solvent and high-pressure CO2 sorption cooperatively soften the matrix, triggering a sharp upward swing in free volume expansion.
FIGURE 4
The location of this anti-plasticization minimum is highly sensitive to the intrinsic flexibility of the polyimide backbone. Specifically, while the minimum FFV increase for the highly flexible 6FDA-ODA/NMP occurs at a low solvent content of 1 wt% (where the swelling drops to a mere 6.73%), it shifts to a higher threshold of 2 wt% for the rigid 6FDA-DAM/NMP matrix (with a minimum swelling of 15.1%). Because 6FDA-ODA possesses highly flexible ether linkages, the localized competitive equilibrium between the residual solvent and CO2 is highly pronounced and easily saturated at minimal solvent contents, whereas the rigid DAM backbone with a bulky methyl side group requires higher solvent constraints to suppress CO2 swelling (). Once these thresholds are observed, cooperative plasticization takes over, driving the swelling up to 20.7% and 15.3% at 4 wt% solvent for the DAM and ODA series, respectively. To quantitatively investigate the linkage flexibility, the standard deviation of the dihedral angle distribution along the imide linkage (σ|ϕ|) was evaluated. Between 0 and 4 wt% THF content, a slight increase in the standard deviation was captured, whereas the NMP series maintained a flat baseline across varying solvent concentrations. This reveals that the smaller, more agile THF molecules actively deform and alter the localized polyimide chain configurations, a phenomenon most dominantly experienced within the flexible 6FDA-ODA network.
These atomistic findings align well with both our experimental results and the pioneering experimental observations of , who postulated that the transition threshold from anti-plasticization to plasticization. Furthermore, both experimental findings highlight that complete solvent evacuation is practically unachievable, retaining lower than 1.0 wt% even after aggressive high-temperature annealing, which further validates why understanding these trace-concentration thresholds computationally is so vital. Collectively, these estimated sub-microscopic structural properties demonstrate quantitative and qualitative agreement with our macroscopic experimental data, including the Tg and d-spacing trends, validating the predictive power of this dual multi-scale approach.
5.5 Sorption predictions of GCMC simulations
Acquiring direct experimental sorption isotherms for the solvent-containing membranes presents significant experimental challenges, primarily due to the extreme difficulty of maintaining precise trace solvent thresholds without triggering premature evaporation during high-pressure testing. However, the reliability of the computational methodology employed herein has been firmly established. In our previous work, this exact GCMC protocol was rigorously validated, demonstrating that the simulated CO2 and CH4 sorption coefficients for the pure 6FDA-DAM matrix match well with experimental measurements (). In terms of polymer packing, while a discrepancy exists between the simulated densities and the current experimental measurements, this variance is due to the distinct physical and methodological differences rather than computational inaccuracy. Specifically, the simulations were performed at 35 °C using shorter polymer chains (), introducing chain-end free volume effects compared to the experimental batches () tested at 23 °C. Furthermore, the experimental films undergo significant thermal annealing (up to 385 °C), inducing a kinetic structural collapse that static packing algorithms cannot fully replicate. Despite this absolute difference, the simulated values perfectly align with the established theoretical baseline density (1.24 g/cm3 (gram per cubic centimeter) validated in our prior work (). Building upon this validated baseline, the GCMC predictions in the current study are confidently utilized as a theoretical diagnostic tool. They serve to isolate the thermodynamic sorption behavior and reveal the complex competitive interactions between penetrants and residual solvents, thereby providing the crucial molecular-level context needed to interpret the macroscopic experimental permeation trends. Therefore, here we provided a methodological synergy between our experimental and computational approaches. While the macroscopic permeation experiments directly capture the ultimate size-sieving (diffusion-dominated) capability of the compacted networks, explicitly simulating these slow diffusion events via Molecular Dynamics in tightly packed glassy polymers is often computationally prohibitive and prone to large uncertainties. Therefore, our computational framework exclusively targeted the thermodynamic aspect of the solution-diffusion mechanism via GCMC simulations. They explicitly reveal how trace solvent molecules occupy pre-defined high-affinity sites, thereby thermodynamically regulating CO2 uptake and the subsequent localized matrix dilation. This localized thermodynamic competition directly dictates the sub-nanometer free volume dimensions, which ultimately governs the kinetic size-sieving behavior observed in our macroscopic permeation experiments.
Grand Canonical Monte Carlo (GCMC) simulations were systematically carried out at 35 °C and 10 bar to quantify the high-pressure sorption coefficients of CO2 and CH4, along with the resulting ideal sorption selectivities across the polyimide matrices (Figures 5a,b). As a general trend, a progressive increase in residual solvent content drives a systematic reduction in CO2 solubility, which correlates with the local densification of the polymer network compiled in Table 4. This decline in gas sorption is primarily governed by a structural saturation mechanism; the remaining solvent molecules accumulate in high-affinity free-volume regions, limiting the space available for CO2 accommodation. Consequently, the gas sorption profile is tightly controlled by both the specific chemical identity and the absolute number of trapped solvent molecules.
FIGURE 5
It is noteworthy that the sorption selectivities plotted in Figure 5b reveal a complex, non-monotonic behavior rather than a simple linear increment, heavily dependent on the trade-off between chain flexibility and solvent features. At a localized threshold of 1 wt% solvent content, certain systems experience a distinct drop or local minimum in sorption selectivity. This structural fluctuation marks the intense localized competition between the penetrant and the solvent molecules before the matrix reorganizes. Beyond this competitive threshold (at 2 wt% and 4 wt% solvent loading), cooperative interactions take over, and the ideal sorption selectivity experiences a steady upward surge. To accurately correlate these computational trends with our macroscopic experimental data, a fundamental distinction in testing parameters must be highlighted. While our experimental data reports overall gas permeability and permselectivity, which encompass the combined effects of both diffusion (D) and sorption (S) coefficients (P = D × S), the GCMC simulation results in Supplementary Table S5 and Figure 5 isolate purely the thermodynamic sorption coefficients and sorption selectivities at 10 bar. At this higher computational pressure, the structural response of the membranes is governed by the cooperative interaction of both the dissolved CO2 penetrants and the residual solvent molecules, especially the above-mentioned threshold value, rather than the solvent alone. In the fully evacuated computational cells (0 wt%), the complete absence of residual solvent molecules deprives the matrix of vital anti-plasticizing rigidifiers or site-blockers. Consequently, the unconstrained free volume pathways become highly vulnerable to high-pressure CO2-induced plasticization. The high penetrant loading at 10 bar dilates these evacuated pathways, which simultaneously expands the thermodynamic capacity for both CO2 and CH4 sorption, thereby explaining why the isolated sorption selectivity at 0 wt% appears lower than the solvent-dense matrices. Nevertheless, this high-pressure sorption affinity at low solvent content acts as a powerful cooperative driver under experimental conditions. As the residual solvent is removed and the polyimide matrix transitions into a highly diffusion-selective network, this enhanced CO2 sorption capacity ensures a higher concentration of penetrant molecules at the membrane upstream interface. Given the strict size-exclusion limits of the compacted matrix, these abundant CO2 molecules diffuse more rapidly and selectively through the narrow interchain voids than the bulkier CH4, ultimately multiplying the overall experimental permselectivity through a synergistic sorption-diffusion mechanism.
Deeper insights into the competitive sorption mechanism are unveiled by tracking the localized positioning of the residual solvents and CO2 around pre-defined sorption sites of polyimide (Supplementary Figure S5). RDFs are used for an in-depth analysis of atomic interactions between penetrants and the polyimide matrices. As represented in Figure 1, RDFs of CO2 around five typical atoms in polyimide chains are selected as follows: the oxygen (O1) and nitrogen (N) in the imide, the fluorine (F) in the -CF3 group, the oxygen (O2) in the ether linkage, and carbon (C) in the–CH3 groups of DAM diamine. The fluorine in the -CF3 group is the least preferential sorption site in each polyimide for both solvents and CO2. Conversely, the localized region corresponding to the imide linkage, situated precisely between the N and O1 sites, emerges as the most dominant preferential sorption epicenter. This steric and electrostatic affinity is clearly demonstrated by the RDF profiles, where the peaks associated with the N and O1 sites display the highest intensities across all simulated systems. Therefore, considering all sites in the rigid 6FDA-DAM matrix, the intensity and spatial positioning of the CO2 g(r) peaks remain remarkably steady across varying THF and NMP concentrations (see an example of N for NMP and THF in Figures 6a,b, respectively). This directly reflects the exceptional structural rigidity of the DAM-based chain architecture. Contrarily, the flexible 6FDA-ODA matrix experiences pronounced structural transformations, particularly localized only at the bridging O2 sites (Figures 6c,d). As the residual solvent content increases, the intensity of the CO2 g(r) peak undergoes a non-monotonic shift, initially decreasing at intermediate solvent thresholds before rising again at higher concentrations for both NMP and THF. This distinct structural fluctuation provides direct atomistic evidence of the shifting continuum between solvent-induced anti-plasticization and penetrant-driven plasticization. Because the ether linkage (O2) represents the high-affinity epicenter for both CO2 and the casting solvents, the flexible 6FDA-ODA backbone adapts its local dihedral configurations to accommodate this crowding. The presence of this flexible ether joint renders the ODA-based matrix significantly more vulnerable to the dual effects of solvent-induced anti-plasticization and subsequent high-pressure CO2 dilation, successfully decoupling the sub-microscopic origin of our experimental and computational transport trends.
FIGURE 6
While our RDF profiles reveal the O2 (ether) site as a second high-affinity epicenter in 6FDA-ODA polyimide, it is important to interpret this finding within the framework of experimental spectroscopy. Time-resolved FTIR studies on polyimides consistently identify imide carbonyls as primary interaction sites (e.g., hydrogen-bond acceptors) (; ) while frequently reporting the ether linkage as unperturbed. This apparent discrepancy between computational and spectroscopic observations stems from methodological differences. In FTIR spectra, the imide carbonyl (C=O) stretching vibrations (1710–1790 cm-1) are highly strong and well-isolated, making interaction-induced vibrational shifts easily resolvable. Contrarily, the asymmetric stretching of the ether (C–O–C) linkage (typically 1200–1250 cm-1) resides in a highly crowded fingerprint region. In 6FDA-based polyimides, this ether band is highly masked by the intense and broad C–F stretching vibrations of the –C(CF3)2– groups (; ). Consequently, potential interaction-induced shifts at the ether site are spectroscopically shadowed, leading to an unperturbed appearance in experimental spectra. Computationally, standard force fields assign a negative partial charge to the ether oxygen, generating a deep electrostatic potential well that dictates an affinity observed in the RDF profiles. Therefore, these GCMC results highlight the electrostatic thermodynamic probability, providing a microscopic perspective that complements the mode-selective capabilities of FTIR spectroscopy.
6 Conclusion
This study proposes to bridge the gap between casting processing history, local macromolecular environments, and high-pressure gas transport mechanisms through a synchronized experimental and computational approach. Experimentally, a systematic thermal treatment protocol implemented across distinct regimes (below boiling point, above boiling point, and near polymer Tg) demonstrated that the physical architecture of polyimide membranes is profoundly conditioned by its casting solvent history. The gradual thermal evaporation of high-boiling solvents (such as NMP) triggers severe macrostructural compaction of the polymer matrix. This collapse of the sub-nanometer free volume network shifts the transport properties from a plasticization-dominated state to an anti-plasticization state or a strict, diffusion-controlled screening regime, where the diffusion paths for the bulkier CH4 molecules are effectively blocked, driving a dramatic surge in experimental permselectivity evaluated at a constant pressure of 4 bar. Complementary molecular simulations executed at an elevated pressure of 10 bar using idealized residual solvent loadings (0–4 wt%) provided crucial sub-microscopic evidence of the fine line where processing thresholds drive or suppress penetrant-induced swelling. It is imperative to note that because of the difference in operational pressures (10 bar for simulations vs. 4 bar for experiments) and the unknown exact mass fraction of the residual solvent in the real membrane samples, these computational predictions are qualitatively, rather than quantitatively, comparable to the experimental results. Nevertheless, they serve as a powerful mechanistic bridge. The 10 bar GCMC models magnify the thermodynamic interactions, explicitly capturing a fierce, localized competition between high-pressure CO2 penetrants and trace amounts of residual solvents. At minimal solvent concentrations depending on backbone rigidity, an anti-plasticization threshold is achieved; the remaining solvent molecules successfully rigidify the matrix and block the preferential sorption sites, specifically the high-affinity imide linkage coordinates (N and O1) and bridging ether joints (O2). However, when the solvent is completely evacuated, the absence of this molecular blockage leaves the highly open free volume pathways vulnerable to aggressive high-pressure CO2-induced plasticization, which dilates the unconstrained channels and alters the isolated thermodynamic sorption selectivity. Furthermore, cross-evaluating the rigid 6FDA-DAM framework against the flexible 6FDA-ODA matrix revealed that chain flexibility dictates the longevity of processing landmarks. While the rigid DAM network resists permanent structural distortion and is governed by a direct balance between penetrant pressure and compaction, the flexible ODA chains preserve a long-lasting thermodynamic “imprint” left by the casting solvent. This structural memory locks the flexible matrix into an expanded configuration that limits its intrinsic sorting efficiency even after the solvent molecules are fully removed. Ultimately, these findings reveal that the overall separation capability of a membrane is a synergistic balance: the enhanced sorption affinity at low solvent contents leads to the accumulation of CO2 molecules at the upstream interface, creating a stronger driving force for these penetrants to rapidly and selectively diffuse through the diffusion-selective matrix channels. This dual multi-scale blueprint offers crucial guidelines for tailoring next-generation polymeric membranes with optimized structural stability and high-pressure performance.
Statements
Data availability statement
The original contributions presented in the study are included in the article/Supplementary Material, further inquiries can be directed to the corresponding author.
Author contributions
DK: Investigation, Writing – review and editing, Data curation, Formal Analysis. SV: Conceptualization, Data curation, Formal Analysis, Investigation, Writing – original draft. MGA: Conceptualization, Funding acquisition, Methodology, Supervision, Writing – review and editing. ŞBTE: Conceptualization, Funding acquisition, Investigation, Methodology, Resources, Supervision, Writing – review and editing.
Funding
The author(s) declared that financial support was received for this work and/or its publication. This work was supported by the Scientific Projects Unit of Istanbul Technical University (Grant# 34479). Computing resources used in this work were provided by the National Center for High-Performance Computing of Turkey (UHeM) under grant# 1003032013.
Conflict of interest
The author(s) declared that this work was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.
Generative AI statement
The author(s) declared that generative AI was used in the creation of this manuscript. Generative AI tools (Gemini) were used solely for only language editing. The AI tools were not used to generate original scientific content, data, analyses, interpretations, or conclusions. All scientific content and responsibility for the manuscript remain with the authors.
Any alternative text (alt text) provided alongside figures in this article has been generated by Frontiers with the support of artificial intelligence and reasonable efforts have been made to ensure accuracy, including review by the authors wherever possible. If you identify any issues, please contact us.
Publisher’s note
All claims expressed in this article are solely those of the authors and do not necessarily represent those of their affiliated organizations, or those of the publisher, the editors and the reviewers. Any product that may be evaluated in this article, or claim that may be made by its manufacturer, is not guaranteed or endorsed by the publisher.
Supplementary material
The Supplementary Material for this article can be found online at: https://www.frontiersin.org/articles/10.3389/frmst.2026.1950898/full#supplementary-material
References
1
AdewoleJ. K.AhmadA. L.IsmailS.LeoC. P.SultanA. S. (2015). Comparative studies on the effects of casting solvent on physico‐chemical and gas transport properties of dense polysulfone membrane used for CO2/CH4 separation. J. Appl. Polym. Sci.132 (27), 1–10. 10.1002/app.42205
2
AhmadM. S.MohshimD. F.NasirR.MannanH. A.MukhtarH. (2018). Effect of solvents on the morphology and performance of polyethersulfone (PES) polymeric membranes material for CO2/CH4 separation. IOP Conf. Ser. Mater Sci. Eng.290 (1), 012074. 10.1088/1757-899X/290/1/012074
3
AlentievA.YampolskiiY.KostinaJ.BondarenkoG. (2006). New possibilities for increasing the selectivity of polymer gas separating membranes. Desalination199 (1–3), 121–123. 10.1016/j.desal.2006.03.027
4
AnsaloniL.MinelliM.Giacinti BaschettiM.SartiG. C. (2015). Effects of thermal treatment and physical aging on the gas transport properties in Matrimid®. Oil and Gas Sci. Technol. – Revue D’IFP Energies Nouvelles70 (2), 367–379. 10.2516/ogst/2013188
5
BakerR. W. (2023). Membrane technology and applications. Wiley, 1–539. 10.1002/9781119686026
6
BalçıkM.AhunbayM. G. (2018). Prediction of CO2-induced plasticization pressure in polyimides via atomistic simulations. J. Memb. Sci.547, 146–155. 10.1016/J.MEMSCI.2017.10.038
7
BerendsenH. J. C.PostmaJ. P. M.van GunsterenW. F.DiNolaA.HaakJ. R. (1984). Molecular dynamics with coupling to an external bath. J. Chem. Phys.81 (8), 3684–3690. 10.1063/1.448118
8
BernardoP.ScorzafaveV.ClariziaG.TocciE.JansenJ. C.BorgognoA.et al (2019). Thin film composite membranes based on a polymer of intrinsic microporosity derived from Tröger’s base: a combined experimental and computational investigation of the role of residual casting solvent. J. Memb. Sci.569 (April 2018), 17–31. 10.1016/j.memsci.2018.10.001
9
BiJ.SimonG. P.YamasakiA.WangC. L.KobayashiY.GriesserH. J. (2000). Effects of solvent in the casting of poly(1-trimethylsilyl-1-propyne) membranes. Radiat. Phys Chem58 (5–6), 563–566. 10.1016/S0969-806X(00)00218-8
10
BosA.PüntI. G. M.WesslingM.StrathmannH. (1999). CO2-induced plasticization phenomena in glassy polymers. J. Memb. Sci.155 (1), 67–78. 10.1016/S0376-7388(98)00299-3
11
BosA.PüntI.StrathmannH.WesslingM. (2001). Suppression of gas separation membrane plasticization by homogeneous polymer blending. AIChE J.47 (5), 1088–1093. 10.1002/aic.690470515
12
BurnsR. L.KorosW. J. (2003). Structure−property relationships for poly(pyrrolone-imide) gas separation membranes. Macromolecules36 (7), 2374–2381. 10.1021/ma0259261
13
ChangK. S.HsiungC. C.LinC. C.TungK. L. (2009). Residual solvent effects on free volume and performance of fluorinated polyimide membranes: a molecular simulation study. J. Phys. Chem. B113 (30), 10159–10169. 10.1021/jp900246p
14
FrenkelD.SmitB.RatnerM. A. (1997). Understanding molecular simulation: from algorithms to applications. Phys. Today50 (7). 23–61. 10.1063/1.881812
15
FuY. J.HuC. C.QuiH. zhiLeeK. R.LaiJ. Y. (2008). Effects of residual solvent on gas separation properties of polyimide membranes. Sep. Purif. Technol.62 (1), 175–182. 10.1016/j.seppur.2008.01.008
16
GaliziaM.ChiW. S.SmithZ. P.MerkelT. C.BakerR. W.FreemanB. D. (2017). 50th anniversary perspective: polymers and mixed matrix membranes for gas and vapor separation: a review and prospective opportunities. Macromolecules50 (20), 7809–7843. 10.1021/acs.macromol.7b01718
17
GuanR.DaiH.LiC.LiuJ.XuJ. (2006). Effect of casting solvent on the morphology and performance of sulfonated polyethersulfone membranes. J. Memb. Sci.277 (1–2), 148–156. 10.1016/j.memsci.2005.10.025
18
HacarliogluP.ToppareL.YilmazL. (2003). Effect of preparation parameters on performance of dense homogeneous polycarbonate gas separation membranes. J. Appl. Polym. Sci.90 (3), 776–785. 10.1002/app.12505
19
HuangY.WangX.PaulD. R. (2006). Physical aging of thin glassy polymer films: free volume interpretation. J. Memb. Sci.277 (1–2), 219–229. 10.1016/J.MEMSCI.2005.10.032
20
IsmailA. F.LornaW. (2002). Penetrant-induced plasticization phenomenon in glassy polymers for gas separation membrane. Sep. Purif. Technol.27 (3), 173–194. 10.1016/S1383-5866(01)00211-8
21
JolyC.Le CerfD.ChappeyC.LangevinD.MullerG. (1999). Residual solvent effect on the permeation properties of fluorinated polyimide films. Sep. Purif. Technol.16 (1), 47–54. 10.1016/S1383-5866(98)00118-X
22
KertikA.WeeL. H.PfannmöllerM.BalsS.MartensJ. A.VankelecomI. F. J. (2017). Highly selective gas separation membrane using in situ amorphised metal–organic frameworks. Energy Environ. Sci.10 (11), 2342–2351. 10.1039/c7ee01872j
23
KhulbeK. (1997). The morphology characterisation and performance of dense PPO membranes for gas separation. J. Memb. Sci.135 (2), 211–223. 10.1016/S0376-7388(97)00138-5
24
KılıçA.Atalay-OralÇ.SirkecioğluA.Tantekin-ErsolmazŞ. B.AhunbayM. G. (2015). Sod -ZMOF/Matrimid® mixed matrix membranes for CO2 separation. J. Memb. Sci.489, 81–89. 10.1016/j.memsci.2015.04.003
25
KostinaJ.BondarenkoG.AlentievA.YampolskiiY. (2006). The influence of conformation composition of polyheteroarylenes on their transport properties. Desalination200 (1–3), 34–36. 10.1016/j.desal.2006.03.232
26
KostinaYu V.BondarenkoG. N.AlentievA.YampolskiiY. (2006). Effect of chloroform on the structure and gas-separation properties of poly(ether imides). Poly Sci. Ser. A48 (1), 32–38. 10.1134/S0965545X06010056
27
KraftschikB.KorosW. J.JohnsonJ. R.KarvanO. (2013). Dense film polyimide membranes for aggressive sour gas feed separations. J. Memb. Sci.428, 608–619. 10.1016/J.MEMSCI.2012.10.025
28
KruczekB.MatsuuraT. (2003). Effect of solvent on properties of solution‐cast dense SPPO films. J. Appl. Polym. Sci.88 (5), 1100–1110. 10.1002/app.12032
29
LeeJ. S.MaddenW.KorosW. J. (2010). Antiplasticization and plasticization of Matrimid® asymmetric hollow fiber membranes. Part B. Modeling. J. Memb. Sci.350 (1–2), 242–251. 10.1016/j.memsci.2009.12.034
30
LiuZ.CaoY.QiuW.KimJ.CampbellZ. S.SchlosserS.et al (2024). Insights on influence of polymer molecular weight on gas sorption, transport and plasticization in glassy 6FDA-DAM polyimide membranes. J. Memb. Sci.712, 123242. 10.1016/J.MEMSCI.2024.123242
31
MacchioneM.JansenJ. C.De LucaG.TocciE.LongeriM.DrioliE. (2007). Experimental analysis and simulation of the gas transport in dense hyflon® AD60X membranes: influence of residual solvent. Polym. Guildf.48 (9), 2619–2635. 10.1016/j.polymer.2007.02.068
32
MichaelsA. S.BixlerH. J. (1961). Flow of gases through polyethylene. J. Poly Sci.50 (154), 413–439. 10.1002/pol.1961.1205015412
33
Mizrahi RodriguezK.LinS.WuA. X.StormeK. R.JooT.GroszA. F.et al (2024). Penetrant-induced plasticization in microporous polymer membranes. Chem. Soc. Rev.53 (5), 2435–2529. 10.1039/d3cs00235g
34
MustoP.RagostaG.MensitieriG.LavorgnaM. (2007). On the molecular mechanism of H2O diffusion into polyimides: a vibrational spectroscopy investigation. Macromolecules40 (26), 9614–9627. 10.1021/ma071385+
35
MustoP.GaliziaM.La MannaP.PannicoM.MensitieriG. (2014). Diffusion and molecular interactions in a methanol/polyimide system probed by coupling time-resolved FTIR spectroscopy with gravimetric measurements. Front. Chem.2, 2. 10.3389/fchem.2014.00002
36
QiuW.ChenC. C.XuL.CuiL.PaulD. R.KorosW. J. (2011). Sub-Tg cross-linking of a polyimide membrane for enhanced CO2 plasticization resistance for natural gas separation. Macromolecules44 (15), 6046–6056. 10.1021/ma201033j
37
RecioR.PalacioL.PradanosP.HernandezA.LozanoA.MarcosA.et al (2007). Gas separation of 6FDA–6FpDA membranes. Effect of the solvent on polymer surfaces and permselectivity. J. Memb. Sci.293 (1–2), 22–28. 10.1016/j.memsci.2007.01.022
38
RoweB. W.FreemanB. D.PaulD. R. (2009). Physical aging of ultrathin glassy polymer films tracked by gas permeability. Polym. Guildf.50 (23), 5565–5575. 10.1016/J.POLYMER.2009.09.037
39
SandersD. F.SmithZ. P.GuoR.RobesonL. M.McGrathJ. E.PaulD. R.et al (2013). Energy-efficient polymeric gas separation membranes for a sustainable future: a review. Polym. Guildf.54 (18), 4729–4761. 10.1016/j.polymer.2013.05.075
40
SeoH.ChaeB.ImJ. H.JungY. M.LeeS. W. (2014). Imidization induced structural changes of 6FDA-ODA poly(amic acid) by two-dimensional (2D) infrared correlation spectroscopy. J. Mol. Struct.1069 (1), 196–199. 10.1016/J.MOLSTRUC.2014.02.012
41
ShaoL.ChungT.WensleyG.GohS.PramodaK. (2004). Casting solvent effects on morphologies, gas transport properties of a novel 6FDA/PMDA-TMMDA copolyimide membrane and its derived carbon membranes. J. Memb. Sci.244 (1–2), 77–87. 10.1016/j.memsci.2004.07.005
42
ShekhawatD.LuebkeD. R.PennlineH. W. (2003). A Review of Carbon Dioxide Selective Membranes, 1200. United States: US department of energy, 9–11.
43
Shiva PrasadN.BabaraoR.MadapusiS.SridharS.ChoudhuryN. R.BhargavaS. K. (2022). Residual solvent induced physical morphology and gas permeation in polyamide-imide membrane: experimental investigation and molecular simulations. Eur. Polym. J.165 (October 2021), 111012. 10.1016/j.eurpolymj.2022.111012
44
SwaidanR.Al-SaeediM.GhanemB.LitwillerE.PinnauI. (2014). Rational design of intrinsically ultramicroporous polyimides containing bridgehead-substituted triptycene for highly selective and permeable gas separation membranes. Macromolecules47 (15), 5104–5114. 10.1021/ma5009226
45
TungK. L.LuK. T.RuaanR. C.LaiJ. Y. (2006). MD and MC simulation analyses on the effect of solvent types on accessible free volume and gas sorption in PMMA membranes. Desalination192 (1–3), 391–400. 10.1016/j.desal.2005.08.018
46
VelioğluS.AhunbayM. G.Tantekin-ErsolmazS. B. (2012). Investigation of CO2-induced plasticization in fluorinated polyimide membranes via molecular simulation. J. Memb. Sci.417–418, 217–227. 10.1016/j.memsci.2012.06.043
47
ViethW. R.SladekK. J. (1965). A model for diffusion in a glassy polymer. J. Colloid Sci.20 (9), 1014–1033. 10.1016/0095-8522(65)90071-1
48
WindJ. D.SirardS. M.PaulD. R.GreenP. F.JohnstonK. P.KorosW. J. (2003). Relaxation dynamics of CO2 diffusion, sorption, and polymer swelling for plasticized polyimide membranes. Macromolecules36 (17), 6442–6448. 10.1021/ma034359u
49
XiL.LvY.FengJ.HuangY.HuangY.YangQ.et al (2024). Synthesis of UV-resistant and colorless polyimide films for optoelectrical applications. NPJ Mater Degrad.8 (1), 6. 10.1038/s41529-023-00422-w
50
ZhangL.FangW.JiangJ. (2011). Effects of residual solvent on membrane structure and gas permeation in a polymer of intrinsic microporosity: insight from atomistic simulation. J. Phys. Chem. C115 (22), 11233–11239. 10.1021/jp2029888
Summary
Keywords
CO2 separation performance, gas separation membranes, molecular simulation, plasticization, residual solvent
Citation
Kahraman D, Velioğlu S, Ahunbay MG and Tantekin-Ersolmaz ŞB (2026) From plasticization to anti-plasticization: the critical role of residual solvent and thermal history on CO2 transport in 6FDA polyimide membranes. Front. Membr. Sci. Technol. 5:1950898. doi: 10.3389/frmst.2026.1950898
Received
28 July 2026
Revised
24 September 2026
Accepted
29 September 2026
Published
10 November 2026
Volume
5 - 2026
Edited by
Aydın Cihanoğlu, Ege University, Türkiye
Reviewed by
Akshay Modi, Indian Institute of Science Education and Research, India
Cosimo Brondi, Universitas Mercatorum Dipartimento di Ingegneria e scienze, Italy
Antonio Baldanza, University of Naples Federico II, Italy
Updates
Copyright
© 2026 Kahraman, Velioğlu, Ahunbay and Tantekin-Ersolmaz.
This is an open-access article distributed under the terms of the Creative Commons Attribution License (CC BY). The use, distribution or reproduction in other forums is permitted, provided the original author(s) and the copyright owner(s) are credited and that the original publication in this journal is cited, in accordance with accepted academic practice. No use, distribution or reproduction is permitted which does not comply with these terms.
*Correspondence: Ş. Birgül Tantekin-Ersolmaz, ersolmaz@itu.edu.tr
ORCID: Duygu Kahraman: orcid.org/0000-0001-9288-332X; Göktuğ Ahunbay: orcid.org/0000-0003-3595-6419; Sadiye Velioğlu: orcid.org/0000-0002-4812-3611; Ş. Birgül Tantekin-Ersolmaz: orcid.org/0000-0003-0620-8948
Disclaimer
All claims expressed in this article are solely those of the authors and do not necessarily represent those of their affiliated organizations, or those of the publisher, the editors and the reviewers. Any product that may be evaluated in this article or claim that may be made by its manufacturer is not guaranteed or endorsed by the publisher.