ORIGINAL RESEARCH article

Front. Sens., 20 October 2026

Sec. Physical Sensors

Volume 7 - 2026 | https://doi.org/10.3389/fsens.2026.1953610

Early warning of PVC overheating in a simulated 10 kV cable trench using thermally induced particulate matter

  • ZW

    Zhaoguo Wu 1

  • QW

    Qian Wang 1

  • QX

    Qianbo Xiao 1

  • SW

    Shuai Wang 2

  • YS

    Yuhuan Shao 3*

  • WG

    Wei Guo 2

  • YL

    Yingkai Long 1

  • HH

    Huixian Huang 4

  • 1. State Grid Chongqing Electric Power Research Institute, Chongqing, China

  • 2. State Grid Beijing Electric Power Research Institute, Beijing, China

  • 3. Chongqing University of Posts and Telecommunications, Chongqing, China

  • 4. State Grid Chongqing Electric Power Company, Chongqing, China

Abstract

Thermally induced particulate matter (TIPM) may provide an indicator of abnormal cable-material heating before combustion. This study combines thermogravimetric analysis, a qualitative comparison with a particle counter, and sensor measurements in a 6 m simulated cable trench. The PVC sample lost approximately 1.6% of its mass below 200 °C. This observation is consistent with low-temperature volatile release but does not identify the emitted species or establish a particle-formation pathway. Five laser particle sensors (LPS), spaced 1 m apart, monitored end-source and central-source configurations at 100 °C–110 °C, 150 °C–160 °C, and 200 °C–210 °C. No sensor response was reported at 100 °C–110 °C in the trench tests. At the two higher temperature ranges, response onset depended on source position and distance. In the reported end-source test at 200 °C–210 °C, N1 responded at 18.31 min and the HCl sensor at 27 min, a difference of 8.69 min. This is a single-run comparison, not a validated lead time to ignition. The spatial response patterns support further evaluation of distributed particle sensing, while replication, quantitative detection thresholds, and field-interference testing are needed before deployment rules can be established.

1 Introduction

10 kV cable trenches are important components of urban power-distribution networks. Failures of the cables they contain can interrupt electricity supply and threaten infrastructure safety (Thai et al., 2024; Zhang et al., 2024; He et al., 2025a).

Cable trenches are often narrow, elongated, and partly enclosed, with restricted ventilation and heat dissipation. Cable insulation and sheath materials, including polyvinyl chloride (PVC), polyethylene (PE), and cross-linked polyethylene (XLPE), can deteriorate under mechanical stress, environmental exposure, and electrical loading (Wu et al., 2025a; Liu et al., 2024; Li et al., 2024). Local overheating or electrical faults may subsequently develop into fires. Detecting these conditions is difficult because early emissions can be weak and their transport depends on trench geometry and airflow (Liu X. et al., 2021; Liu S. et al., 2021; Liao et al., 2025).

The development of an electrical fire sequentially progresses through the early stage of thermal degradation, the stage of smoldering, the stage of combustion, and the stage of open flames. The stage of thermal degradation is characterized by low temperatures and an absence of open flames or dense smoke (Kropotova et al., 2022). During this phase, the insulation materials undergo thermal degradation, producing minute quantities of gas molecules and particles. This stage persists for an extended duration, providing sufficient time for monitoring and intervention. If abnormal conditions of operation are detected early, maintenance personnel can promptly conduct repairs to prevent the occurrence of a fire (Fu et al., 2025).

The conventional monitoring of fires primarily relies on technologies for the sensing of temperature, the detection of smoke, and the detection of characteristic gases; however, each method exhibits specific limitations within complex 10 kV cable trenches. Although the sensing of temperature offers robust capabilities for anti-interference, it experiences a severe lag in time. By the time an alarm triggers, the fire typically advances into the stage of smoldering or the stage of open flames (Zhu et al., 2022; Sugitani et al., 2026). The detection of smoke identifies fires through the effect of light scattering caused by smoke. While cost-effective, this approach primarily targets the dense smoke with large particles present during the middle and late stages of a fire, remaining largely ineffective during the smokeless early stage of thermal degradation (Wang et al., 2025; Cho et al., 2023). The monitoring of characteristic gases, which targets carbon monoxide and alkanes, detects the thermal degradation of materials at an earlier phase but presents distinct shortcomings in practical applications. The initial production of gas remains extremely low and dilutes rapidly within the semi-enclosed and narrow 10 kV cable trenches under the influence of currents from thermal drafts. Furthermore, the molecules of gas are highly susceptible to cross-interference from fluctuations in ambient temperature, levels of humidity, and impurity gases in the background. This susceptibility leads to persistently high rates of missed detections and false alarms, thereby failing to satisfy the requirements for precise early warning (Solórzano et al., 2022; Tang et al., 2022).

To address the limitations of conventional methods for monitoring, academia gradually shifts its focus of research toward early monitoring based on thermally induced particulate matter (TIPM). Upon the heating of insulation materials, the breaking of macromolecular chains releases high concentrations of submicron TIPM, which experiences minimal impact from the dilution of airflow. Numerous scholars continually conduct explorations within this field. He et al. (2025b) investigate the characteristics regarding the emission of TIPM from the insulation materials of polyvinyl chloride within switchgears at different stages of heating. They discover that the response of the laser particle sensor (LPS) occurs significantly earlier than that of conventional sensors for gases. Zhang et al. (2025) study the patterns of thermal degradation for the materials of cables under the stress of coupled electro-thermal conditions, confirming that microscopic particles exhibit a distinct surge in release prior to the initial melting of the material. Vorwerk et al. (2023) examine the features of indication for early fires using distributed sensors with multiple nodes within confined indoor spaces. Their results indicate that the attenuation, which depends on distance, of solid particles with specific sizes serves as a reliable indicator for early warning. Wu et al. (2025b) analyze the behavior of thermal decomposition for the sheaths of polyethylene cables under varying conditions of operation, revealing the mechanism of evolution between microscopic particles and macroscopic fields of temperature. However, current research on TIPM remains limited, and the profiles of diffusion and distribution for this particulate matter within complex trenches are largely unknown. This deficiency results in a lack of a scientific basis for the placement of sensors during engineering installations at actual sites.

To address the demands for the early warning of fires within 10 kV cable trenches, this paper investigates the characteristics of diffusion and distribution for this TIPM within a simulated cable trench. Furthermore, this study conducts a comparative analysis of responses with conventional sensors for gases. Additionally, this research proposes an engineering method for the layout of arrays of LPS, which is tailored to the structural characteristics of the trenches. This approach aims to provide scientific support for the optimization of precise nodes for monitoring.

2 Thermal degradation of PVC

2.1 Thermogravimetric analysis of PVC

PVC was analyzed using a TA SDT Q600 thermogravimetric analyzer in air at a heating rate of 10 °C/min, from room temperature to 600 °C. Figure 1A presents the TG and DTG curves. The first main mass-loss stage spans approximately 200 °C–350 °C, with a DTG peak at 286 °C and a mass loss of 43%. The second stage occurs at approximately 400 °C–500 °C, with a peak at 447 °C and a mass loss of 21%. Literature on PVC associates these stages with dehydrochlorination followed by further decomposition and oxidation of the residual structure (Wang et al., 2018; Yang et al., 2023; Deng et al., 2023). These assignments provide context for the TG/DTG curves; no evolved-gas mass spectra are presented in this study.

FIGURE 1

The enlarged TG curve below 200 °C (Figure 1B) shows a decrease from approximately 99.8%–98.2% (De Bruyne et al., 2024; Deng et al., 2022; Uřičář et al., 2025), corresponding to about 1.6% of the initial sample mass. The small loss is consistent with release of moisture, residual volatiles, or formulation additives. TG alone cannot determine their relative contributions, identify particle composition, or distinguish physical evaporation from chemical reactions. The low-temperature loss motivated the exploratory temperature conditions used below; it does not demonstrate that all released material forms optically detectable particles.

2.2 Formation mechanism of PVC TIPM

Here, TIPM denotes the airborne particles associated with heating the PVC specimen, without assigning a specific chemical composition. Low-temperature mass loss can arise from moisture, residual processing compounds, and formulation additives. In PVC-based cable materials, Sugitani et al. (2026) observed increased volatile emissions around 90 °C–120 °C and identified processing-related residues by GC–MS. This provides a material-specific reason to investigate emissions before the main TG decomposition stage, while leaving the composition of particles in the present experiment unresolved.

After volatile constituents leave the heated material, cooling and sufficient supersaturation may allow condensation onto existing particles or formation of new particles. Coagulation may subsequently alter the size distribution. These processes depend on vapor properties, dilution, residence time, and ambient conditions. A mass-loss signal therefore does not imply a detectable particle concentration at a remote optical sensor, and the available measurements do not establish nucleation rates or phase partitioning.

Dehydrochlorination and subsequent degradation of the PVC backbone are relevant to higher-temperature decomposition (Wang et al., 2018; Yang et al., 2023; Deng et al., 2023). However, the present TG and optical measurements do not establish that polycyclic aromatic hydrocarbons or random chain-scission products dominate emissions at 100 °C–200 °C. Such pathways are not used here as a confirmed explanation of low-temperature particle formation. Figure 2 is intended as a conceptual illustration, not a chemical identification of the measured particles.

FIGURE 2

Studies of other polymer formulations provide context for additive release under thermal stress. Ghanem, Raed A (2015) investigated thermal and photo-initiated TDCP release from polyurethane foam, and Ghanem, Raed A (2025) examined melamine phosphate release from polyurethane foam. These studies support considering additive migration separately from bulk polymer decomposition. Their materials, additives, and exposure conditions differ from those studied here, so their kinetic parameters cannot be transferred directly to cable PVC.

Ghanem, Raed A (2026) reported volatile and nanoscale particulate emission pathways from back-coated textiles subjected to thermal aging, UV irradiation, and abrasion. The nanoscale emissions in that study must be interpreted in the context of those combined stresses; they do not demonstrate heat-only nucleation from PVC. FTIR or GC–MS analysis of evolved gases, together with size-resolved particle-composition measurements, would be needed to distinguish additive release, chemical degradation, and subsequent aerosol formation in the present material.

3 Working principle of laser particle sensor

3.1 Mie scattering theory

To characterize the relationship between particle size and the wavelength of the incident light, a dimensionless size parameter (α) is introduced (Equation 1).

The precise detection of TIPM relies fundamentally on the interaction between light and microscopic particles. Given that the diameter (d) of the particles generated by cable insulation materials during the early stage of thermal degradation is typically of the same order of magnitude as the wavelength (λ) of the detection laser, the light scattering behavior of these particles strictly adheres to Mie scattering theory (Zeng and Xia, 2024). To characterize the relationship between particle size and the wavelength of the incident light, a dimensionless size parameter (α) is introduced. The LPS detects particles through laser-light scattering. For an ideal spherical particle of diameter d illuminated at wavelength λ, Mie theory describes the optical response through the dimensionless size parameter α (Zeng and Xia, 2024):

Because the sensor utilizes a laser source for excitation, the emitted beam exhibits linear polarization. When a linearly polarized laser with a wavelength of λ and an intensity of I0 illuminates at TIPM that is approximated as a sphere, the intensity of the scattered light, I (θ,ϕ), is evaluated at a specific spatial position. This position is defined by the radial distance r from the center of the particle, the scattering angle θ, and the azimuthal angle ϕ between the scattering plane and the plane of incident polarization. The rigorous mathematical expression for this intensity is formulated as follows:

In practical engineering applications, if multiple scattering within the detection cavity is treated as randomly polarized, or if the system employs an unpolarized light model as a computational assumption, the incident light intensity is distributed equally across two orthogonal polarization directions. Consequently, the equivalent scattered light intensity I(θ) simplifies to the following expression (Nie et al., 2025). For unpolarized incident light, or an average over two orthogonal incident polarizations, the corresponding intensity is given by Equation 3 (Nie et al., 2025). This averaging is distinct from multiple scattering, which is not included in the single-particle model.

In Equations 2 and 3, i1 and i2 are the perpendicular and parallel Mie intensity functions. They depend on particle size, relative refractive index, and scattering angle. For a fixed optical geometry, the detected signal depends on both particle abundance and particle optical properties. Converting scattering intensity to mass concentration therefore requires assumptions or calibration concerning size, shape, refractive index, and density. The LPS output is treated as an instrument-reported mass-concentration estimate rather than a chemically specific measurement.

3.2 Sensor detection principles and signal processing

Based on the aforementioned Mie scattering theory, the LPS employed in this study establishes a comprehensive architecture for opto-electro-mechanical coordinated detection. Figure 3 outlines the LPS detection principle. Air carrying suspended particles enters the optical measurement cavity, where particles scatter the incident laser light. A photodetector converts the received light to an electrical signal. Filtering and amplification precede digitization and conversion to a reported concentration (Ge et al., 2026; Xu et al., 2025). This principle explains the sensitivity to particles but does not distinguish PVC-derived emissions from unrelated ambient aerosols. During operation, a constant current source within the sensor drives a laser to emit a stable beam with a specific wavelength into the measurement cavity for optical scattering. Simultaneously, air and potential TIPM from the monitored environment are drawn continuously into the measurement cavity through air channels. The physical intersection between the laser beam and the TIPM within the airflow generates the effect of Mie scattering. Optical receivers, which are positioned at specific angles within the cavity, capture this weak scattered light and convert it into an initial weak current signal. Because this electrical signal is extremely weak and is accompanied by background noise, it requires processing by a subsequent filtering and amplifying circuit to eliminate high-frequency electromagnetic interference and to in-crease the amplitude of the effective signal. Subsequently, the conditioned analog electrical signal is transmitted to a microcontroller unit. This unit digitizes the signal via a built-in module for analog-to-digital conversion and executes a preset algorithm for concentration retrieval. This algorithm accurately converts the discrete electrical signals into a concentration value of the TIPM. This value is ultimately output as a standard digital signal to the upper monitoring computer.

FIGURE 3

3.3 Laser particle sensor sensitivity test

As the core detection instrument for the subsequent polyvinyl chloride (PVC) thermal degradation experiments, the laser particle sensor (LPS) must possess a sensitivity that guarantees the reliable capture of weak signals during the initial pyrolysis stage, ensures data consistency across diverse operating conditions, and adapts to realistic engineering overheating scenarios. Proceeding directly to formal experimentation without prior calibration is prone to inducing measurement deviations, data drift, and inadequate adaptability to specific conditions, which severely compromises the comparative validity of data obtained under varying thermal states. Consequently, aligned with the specific requirements and operating characteristics of the early PVC pyrolysis tests, this study conducts a rigorous sensitivity and performance verification.

Initially, to address the generation characteristics of particulate matter across different size fractions during PVC pyrolysis, a standard particle counter is employed to verify the sensitivity of the LPS. Both the particle counter and the LPS are deployed synchronously within the experimental platform to monitor the suspended particulates generated under identical thermal and environmental baseline conditions. Specifically, the particle counter enumerates particles of various diameters to characterize the particle size distribution, whereas the LPS outputs a continuous signal corresponding to the overall particulate mass concentration. By comparatively analyzing the response onset times and the signal amplification trends of both sensors, the sensitivity and dynamic response capabilities of the LPS during the incipient pyrolysis phase are systematically evaluated. Notably, due to the inherent differences in the physical quantities measured by these two instruments, their outputs are not subjected to absolute numerical comparison; rather, the analysis focuses on the consistency of their evolutionary trends to validate the detection efficacy of the LPS. The specific calibration results are presented in Figure 4.

FIGURE 4

In the reported comparison, both signals remained near baseline during the initial 0–3 min interval at approximately 20 °C. Heating began at 3 min, and both instruments showed an increase approximately 6 min later as the temperature rose toward 100 °C. This qualitative agreement supports detection of a heating-related change under that setup. It does not establish a statistically significant correlation, identical sensitivity, or a universal detection temperature. Differences in dilution and sampling geometry can explain why a local comparison produces a response near 100 °C while the trench tests at 100 °C–110 °C do not.

4 Test platform and test methods

4.1 Simulated cable trench test platform

Given that actual distribution cable trenches typically operate in a semi-enclosed state characterized by restricted internal airflow and a specific longitudinal spatial span, this study constructs a simulated straight cable trench with a total length of 6 m within a laboratory environment. A 6 m long simulated cable trench was constructed with an internal width and height of 0.8 m × 0.8 m. Its geometry was informed by the 2017 State Grid general design for cable lines. The flame-retardant wooden enclosure provides a controlled elongated space for comparing sensor responses. Differences from operational trench materials, cable occupancy, and ventilation are considered in Section 6.

As shown in Figure 5. The monitoring system of the experimental platform comprises an array of LPS, a unit of characteristic gas sensors, and a centralized computer for data acquisition. Along the central axis at the top of the trench, LPS are installed vertically downward at intervals of 1 m. A total of five sensors, designated as N1, N2, N3, N4, and N5, form a linear monitoring array to capture the attenuation of concentration and the patterns of diffusion for the particles along the longitudinal direction of the trench. Simultaneously, the system incorporates a set of highly sensitive electrochemical sensors capable of synchronously monitoring early characteristic gases, including CO, CH4, C2H4, C2H2, and HCl. This integration facilitates a coordinated comparative analysis between the characteristic gases and the TIPM. The source of TIPM combines a piece of PVC material, measuring 40 mm by 40 mm by 10 mm, with a PTC heating plate; additionally, a PT100 temperature sensor detects the temperature of thermal degradation. All sensors connect to the computer, which collects data through a custom program for data acquisition based on LabVIEW software to monitor the temperature of thermal degradation, the concentration of TIPM, and the concentration of characteristic gases in real time. Table 1 presents the parameters of the various sensors employed within this study.

FIGURE 5

TABLE 1

EquipmentResolution and rangeSensing principle
LPS1 μg/m3; 0–2,000 μg/m3Laser-light scattering; mie-based interpretation
CO sensor0.1 ppm; 0–100 ppmElectrochemical, as described in the experimental setup
C2H4/C2H2 sensor0.1 ppm; 0–10 ppmElectrochemical, as described in the experimental setup
CH4 sensor10 ppm; 0–1,000 ppmTransduction principle not specified
HCl sensor0.1 ppm; 0–50 ppmElectrochemical, as described in the experimental setup

Sensor specifications.

4.2 Test method

The test temperatures were selected from the low-mass-loss region and the onset of the first main TG degradation stage. The 100 °C–110 °C condition probes weak low-temperature emissions; 150 °C–160 °C provides an intermediate heating condition; and 200 °C–210 °C approaches the first major degradation region. The lower condition is also supported by reports of volatile release from PVC-based cable materials around 90 °C–120 °C (Sugitani et al., 2026). IEC 60502–2:2014 with Amendment 1:2024 specifies construction, dimensions, and testing for extruded-insulation cables rated 6–30 kV; the three material-heating bands used here are research conditions rather than standard operating limits or prescribed alarm setpoints (IEC, 2014, 2024). For the end-source configuration (L1), the source was positioned below N1 and the gas unit was colocated at N1. This arrangement compares near-source responses while particles travel predominantly in one longitudinal direction.

For the central-source configuration (L2), the source was positioned below N3, allowing transport toward both ends of the trench. The gas unit was placed at N2, 1 m horizontally from the source. L2 denotes the source location, not an additional sensor. The same three temperature conditions were investigated. Because the gas-unit position differs between configurations, comparisons across L1 and L2 include a placement effect as well as any difference in instrument response.

Before each test, forced ventilation was applied at both ends until the sensor readings stabilized near the ambient baseline; the trench was then closed for the measurement. A 15 min baseline was recorded before heating. Data acquisition continued until the farthest sensor showed a distinct response peak or the observation period reached 60 min. Heating was then stopped, the used specimen removed, and the trench ventilated. The three temperature conditions are distinct test conditions, not three replicate runs of one condition. The reported dataset contains one trace per temperature–source-location combination (reported n = 1); no replicate variability is available. Response times are retained on the common acquisition-time basis used in Tables 2 and 3. They describe the reported initial signal rise rather than a validated alarm based on a specified concentration threshold and persistence rule.

TABLE 2

SensorInitial response time (min)Maximum peak concentration (μg/m3)
150 °C–160 °C200 °C–210 °C150 °C–160 °C200 °C–210 °C
N123.418.31448444
N226.0619.67518674
N326.9720.56559653
N428.5621.34518655
N533.8524.49492668

Reported sensor response-onset times and peak concentrations at source location L1.

Values describe one reported run per temperature condition (n = 1), not means; SD and confidence intervals cannot be estimated.

TABLE 3

SensorInitial response time (min)Maximum peak concentration (μg/m3)
150 °C–160 °C200 °C–210 °C150 °C–160 °C200 °C–210 °C
N121.518.24238396
N221.4817.5299609
N318.9516.02590363
N420.2816.91287618
N520.617.73293542

Reported sensor response-onset times and peak concentrations at source location L2.

Values describe one reported run per temperature condition (n = 1), not means; SD and confidence intervals cannot be estimated.

5 Analysis of test results

For the end-source configuration (Figure 6; Table 2), no sensor response was reported at 100 °C–110 °C. At 150 °C–160 °C and 200 °C–210 °C, N1–N5 responded sequentially with increasing distance from the source. At 200 °C–210 °C, the HCl response was reported at 27 min, compared with 18.31 min for N1. The difference is 27–18.31 = 8.69 min for this run. It is neither a mean lead time nor an interval to ignition. N1 response onset changed from 23.40 to 18.31 min between the two higher temperature conditions, while N5 changed from 33.85 to 24.49 min. Peak concentrations did not increase at every node: N1 changed from 448 to 444 μg/m3, whereas N2–N5 increased. Without repeat measurements, neither these differences nor their statistical significance can be established.

FIGURE 6

The reported near-source traces show an initial rise, a decline, and a later increase in particle concentration. This pattern could reflect changes in emission rate, local mixing, deposition, and transport. The signals alone cannot identify a transition from surface-additive release to degradation of deeper polymer layers, so that interpretation is treated as a hypothesis.

An apparent response-front speed was estimated as v_app = Δx/Δt, where Δx is sensor separation and Δt is the difference between reported response-onset times. At L1, the N1–N3 values are 2/(26.97–23.40) = 0.56 m/min and 2/(20.56–18.31) = 0.89 m/min for 150 °C–160 °C and 200 °C–210 °C, respectively. The corresponding N3–N5 values are 2/(33.85–26.97) = 0.29 m/min and 2/(24.49–20.56) = 0.51 m/min. These threshold-dependent timing estimates combine emission, transport, and sensor response; they are not measurements of molecular diffusivity or local airflow velocity.

For the central-source configuration (Figure 7; Table 3), no response was reported at 100 °C–110 °C. At the two higher temperature conditions, N3 above the source responded first, followed by sensors on either side. N3 response onset changed from 18.95 to 16.02 min as the temperature increased. N1 changed from 21.50 to 18.24 min, and N5 from 20.60 to 17.73 min. The earlier onsets are consistent with a change in the combined emission and transport process, but the single traces do not isolate its cause. Peak concentration at N3 decreased from 590 to 363 μg/m3, illustrating that a higher heating temperature does not necessarily produce a higher peak at each sampling position.

FIGURE 7

The central-source traces also show nonmonotonic concentration evolution. Possible causes include time-varying release, unequal transport toward the two ends, and changes in local accumulation or removal. Chemical or depth-resolved degradation processes cannot be inferred uniquely from these concentration curves.

Using the response-onset differences in Table 3, the apparent front speed toward N1 is 2/(21.50–18.95) = 0.78 m/min at 150 °C–160 °C and 2/(18.24–16.02) = 0.90 m/min at 200 °C–210 °C. Toward N5, the corresponding values are 2/(20.60–18.95) = 1.21 m/min and 2/(17.73–16.02) = 1.17 m/min. The two directions therefore show different timing in the reported runs. The N3–N5 estimate does not increase with temperature, so a general claim of faster transport in both directions is not supported. These apparent speeds have no replicate-based uncertainty estimates.

6 Discussion and limitations

A TG balance detects total sample mass loss, whereas an LPS detects scattered light from airborne particles that reach its inlet. Volatile material may remain in the gas phase, and condensable material may be diluted or deposited before sampling. Particle size and refractive index also affect optical response. These distinctions reconcile a small TG loss near 100 °C with no reported trench response at 100 °C–110 °C. The stated 1 μg/m3 display resolution does not define the minimum detectable concentration. The current data cannot separate transport losses from instrument detection limits or establish a universal temperature threshold.

The measurements are exploratory: each temperature–location condition is represented by one reported trace. Sensors N1–N5 sample different positions within a shared run and are not independent experimental replicates. SD, confidence intervals, and statistical significance for response times or peak concentrations cannot be inferred from these spatial measurements. Independent repeated trials, with at least three runs per condition as an initial design and a sample size chosen for the desired precision, are required. Future testing should define the response threshold and persistence duration, report background noise and sampling intervals, and treat nonresponses within the observation period explicitly rather than assigning artificial response times.

Operational trenches contain dust and aerosols unrelated to PVC heating. Humidity can change particle water uptake and light scattering, while inlet or optical-surface contamination can cause drift. Li et al. (2023) investigated combined dual-wavelength scattering and extinction to distinguish fire aerosols from nuisance sources. This supports evaluating additional optical information, but does not establish the same discrimination performance for the LPS used here. A practical validation sequence is to characterize dust and humidity backgrounds, set baseline-adjusted concentration and persistence criteria, and assess confirmation across neighboring particle sensors and gas or temperature channels. Candidate thresholds should be evaluated on separate overheating and nuisance-source trials. Size-selective inlets and dual-wavelength sensing should also be checked for losses of relevant PVC-derived particles.

The PTC-heated PVC coupon does not reproduce a complete energized cable. Metal-core heat conduction, jacket thickness and curvature, insulation layering, electrical loading, aging, and possible metal-mediated reactions may change its heating and emission behavior. The wooden enclosure also differs from operational trench materials and cable occupancy. The next validation step is a comparison of the coupon with intact cable sections at matched measured jacket temperatures, followed by loaded-cable tests that record conductor and surface temperatures separately. The end-source and central-source configurations describe source placement and transport direction, rather than controlled one-ended and two-ended ventilation.

For deployment, D_max denotes the largest source-to-sensor distance that meets a chosen detection-time requirement and false-alarm criterion under representative adverse conditions. Distributed-node measurements have shown that source distance affects both the strength and propagation of early fire indicators (Vorwerk et al., 2023). D_max should therefore be established by moving the source between nodes, testing both transport directions, and retaining the least favorable validated coverage. In a straight unobstructed run with validated coverage in both directions, interior spacing no greater than 2D_max and end coverage no greater than D_max provide a geometric coverage condition. These relations do not yield a numerical spacing recommendation from the present dataset; the 1 m spacing used here remains an experimental configuration.

Further validation should use a fresh specimen for each independent run and begin with at least three runs per temperature–location condition, extending the sample size as needed for precision. A common response rule and sampling interval should be fixed before comparing sensors. Mean response times, standard deviations, and confidence intervals should then be calculated from independent runs, with nonresponses reported separately. Instrument characterization should record the gas-channel transduction principles, quantify particle-sensor baseline noise and response limits, and pair gas analysis with size-resolved particle sampling. These measurements would test the proposed mechanism and determine whether the observed timing advantage is repeatable.

7 Conclusion

To address the critical need for early fire warning in distribution cable trenches, this study systematically investigates the emission mechanisms, diffusion characteristics, and concentration evolution of thermally induced particulate matter through comprehensive material thermal analysis and simulated trench experiments. The findings establish a reliable temperature window and microscopic generation mechanism for incipient warning, demonstrating that although polyvinyl chloride cable insulation undergoes only a minimal mass loss of 1.6 percent below 200 °C, dehydrochlorination and random chain scission mechanisms compel copious low-molecular-weight volatiles to escape and condense into suspended aerosols. This low-temperature nucleation process provides a robust material basis for extremely early detection. Prior to macroscopic application, rigorous synchronous calibration against a standard particle counter confirmed that the laser particle sensor possesses exceptional baseline stability and dynamic tracking capabilities, validating its core monitoring efficacy. Building upon this equipment reliability, comparative experiments within the simulated trench reveal that the optical sensor significantly outperforms conventional characteristic gas sensors, advancing the initial alarm time by up to 8.69 min under a 200 °C fault condition. Furthermore, continuous monitoring elucidates the complex spatiotemporal evolutionary patterns of the particulate matter, characterized by an initial rapid concentration surge, a subsequent brief decline, and a final gradual increase, which objectively reflects the physical transition from superficial volatile release to deep continuous thermal degradation. The spatial migration of these particles within the confined trench is highly nonlinear and asymmetric, manifesting as decelerated diffusion during unidirectional end-faults and pronounced asymmetry during bidirectional mid-trench faults, with elevated heating temperatures consistently accelerating the overall spatial diffusion process. Ultimately, this research bridges the microscopic generation mechanisms with macroscopic diffusion behaviours, offering a solid theoretical foundation and empirical data support for optimizing the deployment of highly sensitive early fire monitoring sensor arrays in complex underground power infrastructure.

Statements

Data availability statement

The original contributions presented in the study are included in the article/Supplementary Material, further inquiries can be directed to the corresponding author.

Author contributions

ZW: Conceptualization, Funding acquisition, Writing – review and editing. QW: Methodology, Writing – review and editing. QX: Investigation, Writing – review and editing. SW: Project administration, Writing – review and editing. YS: Conceptualization, Methodology, Writing – original draft, Writing – review and editing. WG: Resources, Writing – review and editing. YL: Supervision, Writing – review and editing. HH: Supervision, Writing – review and editing.

Funding

The author(s) declared that financial support was received for this work and/or its publication. This research was funded by the Science and Technology Project of State Grid Corporation of China Headquarters, grant number 520201250016–159-ZN.

Conflict of interest

Author HH was employed by State Grid Chongqing Electric Power Company.

The remaining author(s) declared that this work was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.

Generative AI statement

The author(s) declared that generative AI was not used in the creation of this manuscript.

Any alternative text (alt text) provided alongside figures in this article has been generated by Frontiers with the support of artificial intelligence and reasonable efforts have been made to ensure accuracy, including review by the authors wherever possible. If you identify any issues, please contact us.

Publisher’s note

All claims expressed in this article are solely those of the authors and do not necessarily represent those of their affiliated organizations, or those of the publisher, the editors and the reviewers. Any product that may be evaluated in this article, or claim that may be made by its manufacturer, is not guaranteed or endorsed by the publisher.

Supplementary material

The Supplementary Material for this article can be found online at: https://www.frontiersin.org/articles/10.3389/fsens.2026.1953610/full#supplementary-material

References

  • 1

    ChoJ.-H.LeeI.-B.JeongW.-S.LeeB.-J. (2023). A study on the fire detection and smoke removal in underground utility tunnel using CFD. IEEE Access11, 104485–104504. 10.1109/access.2023.3316881

  • 2

    De BruyneA.CérdanK.O’RourkeG.StuyckW.LeindersJ.DenayerM.et al (2024). Evaluation of green biobased plasticizers in poly(vinyl chloride): Sustainability, thermal behavior, mechanical properties, and durability. ACS Appl. Polym. Mater.6, 6831–6842. 10.1021/acsapm.4c00809

  • 3

    DengT.LiS.JiaP.YaoN.DingH.XuL.et al (2022). Self-plasticized PVC prepared by introducing fatty acid to the PVC with triglycidyl isocyanurate as an intermediate bridge. ACS Omega7, 35694–35704. 10.1021/acsomega.2c03655

  • 4

    DengJ.YuK.-L.WangC.-P.ChenL.-J.LyuH.-F.ShuC.-M. (2023). Pyrolysis mechanism of different thermal aging of PVC insulation copper cable for home decoration. Thermochim. Acta729, 179611. 10.1016/j.tca.2023.179611

  • 5

    FuH.QiuL.AiY.YangB.DuF. (2025). Fire hazard detection for power cable tunnel. Sensors Mater.37, 2185. 10.18494/sam5604

  • 6

    GhanemR. A. (2015). Kinetics of thermal and photo-initiated release of tris (1,3-dichloro-2-propyl) phosphate (TDCP) flame retardant from polyurethane foam materials. Journal of Environmental Science and Health, Part A37 (8), 855–865. 10.1080/10934529.2015.1019807

  • 7

    GhanemR. A. (2025). Kinetics release of melamine phosphate from polyurethane foam: Implications for human exposure and environmental stability. J. Hazard. Mater.495, 139057. 10.1016/j.jhazmat.2025.139057

  • 8

    GhanemR. A. (2026). Thermal–UV synergy accelerates HBCD emissions from back-coated textiles via volatile and nanoscale particle pathways. Journal of Environmental Science and Health, Part A61 (6), 410–420. 10.1080/10934529.2026.2655126

  • 9

    GeT.ZhangG.SunW.ZhuJ.BaoY.ShenW. (2026). Optical system design for a high-sensitivity optical particle counter. Meas. Sci. Technol.37, 225201. 10.1088/1361-6501/ae6e5c

  • 10

    HeW.YouY.WuZ.HouZ.LiuX.RenX.et al (2025a). Time‐domain computation of propagation characteristics of partial discharge in cross‐linked polyethylene high‐voltage cable incorporating modified frequency‐dependent parameters. High. Volt.11, 421–433. 10.1049/hve2.70094

  • 11

    HeW.CaiZ.WuZ.ShaoY.WangQ.LongY.et al (2025b). Investigation into the detection of polyvinyl chloride pyrolysis particles in 10-kV switchgear using a laser particle sensor. IEEE Trans. Instrum. Meas.74, 1–11. 10.1109/tim.2025.3595252

  • 12

    KropotovaS. S.KuznetsovG. V.StrizhakP. A. (2022). Identifying products of pyrolysis and combustion of materials at incipient stages of fires. Fire Saf. J.132, 103643. 10.1016/j.firesaf.2022.103643

  • 13

    LiK.LiuG.YuanH.ChenY.DaiY.MengX.et al (2023). Dual-wavelength smoke detector measuring both light scattering and extinction to reduce false alarms. Fire6 (4), 140. 10.3390/fire6040140

  • 14

    LiH.CaiJ.ChenP.ZhangJ.GuoW.PanZ.et al (2024). Effect of moisture on the electric field and breakdown voltage of XLPE cable interconnectors. AIP Adv.14, 115221. 10.1063/5.0226274

  • 15

    LiaoX.LiP.WangZ.FengY.WeiJ. (2025). Rapid and sensitive detection of 2-Ethylhexanol vapor utilizing mesoporous neodymium-doped indium oxide for real-time monitoring of overheated electrical cables. Anal. Chem.97, 7476–7482. 10.1021/acs.analchem.5c00307

  • 16

    LiuX.HouD.JiJ.ZhuH. (2021). Experiment and numerical simulation of cable trench fire detection. Case Stud. Therm. Eng.28, 101338. 10.1016/j.csite.2021.101338

  • 17

    LiuS.FifieldL. S.BowlerN. (2021). Aging mechanisms of filled cross-linked polyethylene (XLPE) cable insulation material exposed to simultaneous thermal and gamma radiation. Radiat. Phys. Chem.185, 109486. 10.1016/j.radphyschem.2021.109486

  • 18

    LiuC.HouY.DuanZ.ShangR.WangK.ChenD. (2024). Underground power cable fault detection and localization based on the spectrum of propagation functions. IEEE Trans. Instrum. Meas.73, 1–11. 10.1109/tim.2024.3453315

  • 19

    NieW.WanJ.XuC.PengH.DouY.LiH. (2025). High-precision measurement of respirable coal dust mass concentration: a dual-wavelength complementary laser optical sensor approach based on Mie scattering. Opt. Lasers Eng.186, 108766. 10.1016/j.optlaseng.2024.108766

  • 20

    SolórzanoA.EichmannJ.FernándezL.ZiemsB.Jiménez-SotoJ. M.MarcoS.et al (2022). Early fire detection based on gas sensor arrays: multivariate calibration and validation. Sensors Actuators B Chem.352, 130961. 10.1016/j.snb.2021.130961

  • 21

    SugitaniM.TanakaW.HondaH.HirotaT.HiguchiM.TakahashiT.et al (2026). Unintended processing-related volatile markers for early-stage overheating of PVC-based cable materials. ACS Appl. Electron. Mater.8, 1650–1658. 10.1021/acsaelm.5c02339

  • 22

    TangY.ZhaoY.LiuH. (2022). Room-temperature semiconductor gas sensors: challenges and opportunities. ACS Sensors7, 3582–3597. 10.1021/acssensors.2c01142

  • 23

    ThaiH.-D.LeN.-B.-V.LeeD.HuhJ.-H. (2024). A survey of electrical fire causes assessment technology. IEEE Access12, 145378–145392. 1–1. 10.1109/access.2024.3437175

  • 24

    UřičářJ.ChodounskáA.BenešováV.BrožekJ.KalouskováR. (2025). Coupled thermogravimetric analysis-potentiometric titration for complex analysis of poly(vinyl chloride) thermal stability. ACS Meas. Sci. Au5, 70–73. 10.1021/acsmeasuresciau.4c00090

  • 25

    VorwerkP.KelleterJ.MüllerS.KrauseU. (2023). Distance-based analysis of early fire indicators on a new indoor laboratory dataset with distributed multi-sensor nodes. Fire6, 323. 10.3390/fire6080323

  • 26

    WangZ.WeiR.WangX.HeJ.WangJ. (2018). Pyrolysis and combustion of polyvinyl chloride (PVC) sheath for new and aged cables via thermogravimetric analysis-fourier transform infrared (TG-FTIR) and calorimeter. Materials11, 1997. 10.3390/ma11101997

  • 27

    WangY.LiQ.ZhangJ.YinC.ZhangQ.ShiY.et al (2025). A gas detection system combined with a global extension extreme learning machine for early warning of electrical fires. Sensors Actuators B Chem.423, 136801. 10.1016/j.snb.2024.136801

  • 28

    WuZ.WangQ.XiaoQ.WuK.FuQ.HuangH.et al (2025a). Study on the effect of environmental humidity on the thermal decomposition characteristics of PVC outer sheath of high-voltage cables. Discov. Appl. Sci.7, 862. 10.1007/s42452-025-07568-z

  • 29

    WuZ.WangQ.HuangH.LiY.KuangY.XiangH.et al (2025b). Research on the thermal decomposition characteristics of PE outer sheath of high-voltage cables under different humidity levels. Energies18, 3537. 10.3390/en18133537

  • 30

    XuC.NieW.PengH.LiH.WanJ. (2025). Enhancing dust concentration monitoring in high particulate matter environments: a dual-light source particulate matter sensor approach based on Mie scattering. Sensors Actuators A Phys.387, 116348. 10.1016/j.sna.2025.116348

  • 31

    YangS.WangY.ManP. (2023). Kinetic analysis of thermal decomposition of polyvinyl chloride at various oxygen concentrations. Fire6, 404. 10.3390/fire6100404

  • 32

    ZengJ.XiaJ. (2024). Light scattering method for aerosol sizing based on machine learning. ACS Sensors9, 1208–1217. 10.1021/acssensors.3c02009

  • 33

    ZhangZ.ZouL.YangH.HanZ. (2024). Prediction of ceiling temperature rise in high-voltage cable trenches with identification of ignition points. Fire7, 316. 10.3390/fire7090316

  • 34

    ZhangP.HuangX.SuJ.LiuZ.PangX.WangZ.et al (2025). Research on diagnostic methods for gas generation due to degradation of cable PVC materials under electrical and thermal stress. Polymers17, 3021. 10.3390/polym17223021

  • 35

    ZhuH.JiJ.NieJ. (2022). Early fire evolution and alarm characteristics of cable fires in long and narrow spaces. Fire Saf. J.131, 103627. 10.1016/j.firesaf.2022.103627

Summary

Keywords

10 kV cable trench, gas sensor, laser particle sensor (LPS), polyvinyl chloride (PVC), thermally induced particulate matter (TIPM)

Citation

Wu Z, Wang Q, Xiao Q, Wang S, Shao Y, Guo W, Long Y and Huang H (2026) Early warning of PVC overheating in a simulated 10 kV cable trench using thermally induced particulate matter. Front. Sens. 7:1953610. doi: 10.3389/fsens.2026.1953610

Received

31 July 2026

Revised

28 September 2026

Accepted

28 September 2026

Published

20 October 2026

Volume

7 - 2026

Edited by

Bing Sun, Nanjing University of Posts and Telecommunications, China

Reviewed by

Zhi Li, Chongqing Jiaotong University, China

Raed Ghanem, Al al-Bayt University Faculty of Science, Jordan

Updates

Copyright

*Correspondence: Yuhuan Shao,

Disclaimer

All claims expressed in this article are solely those of the authors and do not necessarily represent those of their affiliated organizations, or those of the publisher, the editors and the reviewers. Any product that may be evaluated in this article or claim that may be made by its manufacturer is not guaranteed or endorsed by the publisher.

Outline

Figures

Cite article

Copy to clipboard


Export citation file


Share article

Article metrics